MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SEKISUI SPI KYDEX® 6513 Thermoplastic
Categories: Polymer; Thermoplastic

Material Notes: Integral "Frost" low heat release aviation sheet

KYDEX® 6513 is a proprietary, innovative, high performance thermoplastic sheet specifically formulated to meet the safety needs of the aviation industry while elevating aviation interior aesthetic. Color is filtered through frost-like finish to extend luxe design. Hues shift with movement of passenger or part, defining geometry and plane. KYDEX® 6513 is ideal to use with LED lighting, yet dynamic on its own.

KYDEX® 6513 meets all fire retardancy requirements set forth in Federal Aviation Regulations 25.853 paragraphs (a) and (d) (old (c)) including low heat release (65/65) in the OSU rate of heat release test. Its excellent properties make it the ideal material to form two and three-dimensional aircraft components.

Suggested Applications:

  • Seat parts
  • Armrests
  • Passenger service units
  • Kick panels
  • Bulkhead laminates
  • Life vest shrouds
  • Tray tables
  • Accent pieces
  • Window shades
  • Molding strips
  • Monitor shrouds

Features:

  • Available in P-3 texture and thicknesses from 0.71 mm (0.028 in) to 3.18 mm (0.125 in)
  • Meets the stringent requirements of FAR 25.853 paragraph (d) in all thicknesses and colors
  • Easy to fabricate with crisp detail, minimal rejects, and effect integrity
  • Can be formed on all standard presses and cut on all standard die-cutting machines
  • Easy to clean with aggressive cleaners and citrus-based cleaners (avoid ammoniated cleaners)
  • Secondary operations include: machining, sawing, blanking, punching, etc., are easily performed

Values based upon 3.18 mm (0.125 in) sheet unless otherwise specified

Information provided by Sekisui Polymer Innovations

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.48 g/cc1.48 g/ccASTM D792
Moisture Absorption 0.0800 %
@Time 86400 sec
0.0800 %
@Time 24.0 hour
ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 108108ASTM D785
Tensile Strength 53.3 MPa7730 psiASTM D638
Tensile Modulus 3.358 GPa487.0 ksiASTM D638
Flexural Strength 82.7 MPa12000 psiASTM D790
Flexural Modulus 3.358 GPa487.0 ksiASTM D790
Compressive Yield Strength 75.8 MPa11000 psiASTM D695
Compressive Modulus 3.303 GPa479.1 ksiASTM D695
Ultimate Bearing Strength 256.5 MPa37200 psiASTM D953
Bearing Yield Strength 53.3 MPa7730 psi4% deflection; ASTM D953
Shear Strength 56.5 MPa8190 psiASTM D732
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength >= 22.4 kV/mm>= 569 kV/inoil; ASTM D149
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Transverse to Flow 58.3 µm/m-°C32.4 µin/in-°FASTM D831
Deflection Temperature at 1.8 MPa (264 psi) 78.3 °C173 °FAnnealed; ASTM D648
 
Descriptive Properties
Flammability<65 kW/m²FAR 25.853(d) Part IV; OSU Heat Release, peak; all thicknesses
 <65 kW-min/m²FAR 25.853(d) Part IV; OSU Heat Release, 2-min total; all thicknesses
 Dmax<200FAR 25.853(d) Part V; NBS Smoke Density; all thicknesses
 PassFAR 25.853(a)(i); Vertical Burn, 60 sec; all thicknesses
 PassFAR 25.853(a)(ii); Vertical Burn, 12 sec; all thicknesses

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
SEKISUI SPI KYDEX® 410 ABS/PVC
SEKISUI SPI KYDEX® 430 ABS/PVC
SEKISUI SPI KYDEX® 110 Polymer Alloy Sheet
SEKISUI SPI KYDEX® 100 Polymer Alloy Sheet
SEKISUI SPI KYDEX® 2200LT Thermoplastic

PSEKIS043 / 185868

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.