MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Envalior Arnite® T06 202 XL (T-X01151) PBT (European Grade)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Unreinforced, Molded

Material Notes: Arnite resins are engineered to provide specific performance in applications where DSM technology can offer value.

Arnite Molding resins:

  • Standard Unfilled and Reinforced materials
  • High modulus Flame retardant grades
  • Easy molding FR grades for connectors
  • Toughened unfilled materials for durability
  • High modulus, tight specification for critical auto components
  • Toughened reinforced resins
  • Low outgassing grades for reflector surfaces

Arnite extrusion resins: Specialized materials for specific uses

  • PET for medical applications
  • Loose buffer Optical fiber tubing
  • PET for stock shapes

Applications

  • Automotive:Connectors, sensors and E&E parts, Exterior fittings, Gear housings and motors, Brake valve bodies
  • Electrical & Electronic: Telecoms and IT connectors, Bobbins, Low voltage Power distribution, E-motor components, Lightings and Lamp fittings
  • Consumer Durables: Small Appliances
  • Other: Optical fiber tubing

Information provided by DSM.

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.30 g/cc0.0470 lb/in³ISO 1183
Water Absorption 0.45 %0.45 %Sim. to ISO 62
Moisture Absorption at Equilibrium 0.18 %0.18 %Humidity Absorption; Sim. to ISO 62
Melt Flow 39 g/10 min
@Load 2.16 kg,
Temperature 250 °C
39 g/10 min
@Load 4.76 lb,
Temperature 482 °F
Calculated from Volume Flow Rate of 30 cm3/10min.; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 58.0 MPa8410 psiISO 527-1/-2
Tensile Stress at Strain 31.0 MPa
@Strain 50 %
4500 psi
@Strain 50 %
ISO 527-1/-2
Elongation at Break 50 %50 %ISO 527-1/-2
Elongation at Yield 4.0 %4.0 %ISO 527-1/-2
Tensile Modulus 2.70 GPa392 ksiISO 527-1/-2
Charpy Impact Unnotched  NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.500 J/cm²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.500 J/cm²
@Temperature 23.0 °C
2.38 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant  3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
IEC 60250
 3.5
@Frequency 100 Hz
3.5
@Frequency 100 Hz
IEC 60250
Dielectric Strength 27.0 kV/mm686 kV/inIEC 60243-1
Dissipation Factor  0.0020
@Frequency 100 Hz
0.0020
@Frequency 100 Hz
IEC 60250
 0.020
@Frequency 1e+6 Hz
0.020
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 >= 600 V>= 600 VPLC 0; UL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 70.0 µm/m-°C
@Temperature 20.0 °C
38.9 µin/in-°F
@Temperature 68.0 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature 20.0 °C
38.9 µin/in-°F
@Temperature 68.0 °F
ISO 11359-1/-2
Melting Point 225 °C437 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 170 °C338 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C140 °FISO 75-1/-2
Flammability, UL94  HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
IEC 60695-11-10
 HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
IEC 60695-11-10
 
Descriptive Properties
Injection MoldingYes
Release AgentYes
Without FillersYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Envalior Arnite® T06 202 /A PBT
Envalior Arnite® T06 202 PBT (European and Asian Grade)
Envalior Arnite® TM4 440 (PBT+PET)-MD20
BASF Ultradur® B 2550 PBT
Barlog Plastics KEBAFORM C 901 VT POM Copolymer unreinforced, antistatic

PDSMEU340 / 31291

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.