MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Titanium Grade 1, Annealed
Categories: Metal; Nonferrous Metal; Titanium Alloy; Unalloyed/Modified Titanium

Material Notes: Information provided by Allvac and the references.

Applications: Airframe components, cryogenic vessels, heat exchangers, CPI equipment, condenser tubing, pickling baskets. Sample was annealed 2 hr at 700°C..

Forms typically available: billet, bar, plate, sheet, strip, rod, wire, extrusions, tubing.

Titanium Grades 1,2,3,4,7,11,and 12 are all considered unalloyed and have similar mechanical properties.

Key Words: UNS R50250; ASTM Grade 1, CP titanium, C.P. titanium alloy
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 4.51 g/cc0.163 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 120120
Hardness, Knoop 132132Estimated from Brinell.
Hardness, Rockwell B 9090
Hardness, Vickers 122122Estimated from Brinell.
Tensile Strength 152 MPa
@Temperature 316 °C
22000 psi
@Temperature 601 °F
Tensile Strength, Ultimate 330 MPa47900 psi
Tensile Strength, Yield 240 MPa34800 psi
Elongation at Break 30 %30 %
Tensile Modulus 100 GPa14500 ksi
Modulus of Rigidity 38.6 GPa5600 ksi
Compressive Yield Strength 340 MPa49300 psi
Poissons Ratio 0.340.34
Shear Modulus 38.0 GPa5510 ksi
Charpy Impact 140 J103 ft-lbV-notch
Bend Radius, Minimum 2.0 t
@Thickness >=1.80 mm
2.0 t
@Thickness >=0.0709 in
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000450 ohm-cm0.0000450 ohm-cm
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 325 J/g140 BTU/lbHigh Purity Ti.
CTE, linear  8.35 µm/m-°C
@Temperature 15.0 °C
4.64 µin/in-°F
@Temperature 59.0 °F
 8.60 µm/m-°C
@Temperature 20.0 - 93.0 °C
4.78 µin/in-°F
@Temperature 68.0 - 199 °F
 9.20 µm/m-°C
@Temperature 200 °C
5.11 µin/in-°F
@Temperature 392 °F
 19.9 µm/m-°C
@Temperature 20.0 °C
11.1 µin/in-°F
@Temperature 68.0 °F
perpendicular
Specific Heat Capacity 0.520 J/g-°C0.124 BTU/lb-°F
 0.560 J/g-°C
@Temperature 200 °C
0.134 BTU/lb-°F
@Temperature 392 °F
 0.620 J/g-°C
@Temperature 400 °C
0.148 BTU/lb-°F
@Temperature 752 °F
 0.690 J/g-°C
@Temperature 600 °C
0.165 BTU/lb-°F
@Temperature 1110 °F
Thermal Conductivity 16.0 W/m-K111 BTU-in/hr-ft²-°F
Melting Point <= 1670 °C<= 3040 °F
Liquidus 1670 °C3040 °F
Beta Transus 888 °C1630 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.30
@Temperature 710 °C
0.30
@Temperature 1310 °F
High purity Ti
Reflection Coefficient, Visible (0-1) 0.560.56High purity Ti; visible light.
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.10 %<= 0.10 %
Hydrogen, H <= 0.015 %<= 0.015 %
Iron, Fe <= 0.20 %<= 0.20 %
Nitrogen, N <= 0.030 %<= 0.030 %
Other, total <= 0.30 %<= 0.30 %
Oxygen, O <= 0.18 %<= 0.18 %
Titanium, Ti 99.5 %99.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Grade 1
Titanium Grade 2, Annealed
Titanium Grade 2
TIMET TIMETAL® 35A CP Titanium (ASTM Grade 1)
Titanium Grade 4

MTU011 / 14258

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.