MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Thermal Ceramics Therm-O-Seal Insulating Cements
Categories: Ceramic

Material Notes: Therm-O-Seal Insulating Cement is composed of expanded vermiculite granules and unique binders, which mix readily with water to create highly plastic, non-corrosive cement with outstanding adhesion. Especially formulated for ease in troweling, Therm-O-Seal Insulating Cement adheres well to all types of surfaces and may be applied to heat equipment for minor repairs.

Features:

  • Finishing cement recommended for temperatures up to 1400°F
  • Finishing cement provides a strong protective coating for other insulation materials
  • Insulating cement recommended for temperatures up to 1800°F
  • Insulating cement is a non-corrosive cement with outstanding adhesion
  • Fibrous adhesive maximum service temperature 1200°F
  • No asbestos fibers
  • Fast setting compound
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 0.513 g/cc0.0185 lb/in³dry
    Loss On Ignition 1.8 %1.8 %
     
    Thermal PropertiesMetricEnglishComments
    Thermal Conductivity  0.110 W/m-K
    @Temperature 204 °C
    0.760 BTU-in/hr-ft²-°F
    @Temperature 400 °F
    ASTM C201
     0.140 W/m-K
    @Temperature 427 °C
    0.970 BTU-in/hr-ft²-°F
    @Temperature 800 °F
    ASTM C201
     0.180 W/m-K
    @Temperature 649 °C
    1.25 BTU-in/hr-ft²-°F
    @Temperature 1200 °F
    ASTM C201
     0.225 W/m-K
    @Temperature 871 °C
    1.56 BTU-in/hr-ft²-°F
    @Temperature 1600 °F
    ASTM C201
    Maximum Service Temperature, Air 982 °C1800 °F
     
    Component Elements PropertiesMetricEnglishComments
    Al2O3 8.0 %8.0 %
    Alkalis 3.2 %3.2 %
    CaO 27.7 %27.7 %
    Fe2O3 4.2 %4.2 %
    MgO 10 %10 %
    SiO2 44 %44 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Thermal Ceramics V-19 Block Insulation
    LATI LATISHIELD 87/28-06A Polycarbonate E.M.I. Shielding Plastic
    Centro Plastica CiPiTENE® Recycled High Density Polyethylene Granules

    CTHERM256 / 2576

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.