MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

RSP Technology RSA-4019 AE Aluminum Super Alloy
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 4000 Series Aluminum Alloy

Material Notes: Precision Equipment, High Strength - High Temp

RSP Technology develops, produces and sells aluminum super alloys with high end properties. By using its own Meltspinning process, ultra fast cooling rates can be reached, converting more than 1 million degrees per second. As a result very fine nanostructured alloys with new functionalities are being developed and produced.

Information provided by RSP Technology BV

Key Words: AA4019, Aluminium 4019
Vendors: RSP Technology – Aluminum as strong as Titanium For more information contact: +31 (0)596 632 300 or visit www.rsp-technology.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.75 g/cc0.0994 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 140140
Tensile Strength, Ultimate 400 MPa58000 psi
 175 MPa
@Temperature 300 °C,
Time 3.60e+6 sec
25400 psi
@Temperature 572 °F,
Time 1000 hour
 250 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
36300 psi
@Temperature 482 °F,
Time 1000 hour
 330 MPa
@Temperature 200 °C,
Time 3.60e+6 sec
47900 psi
@Temperature 392 °F,
Time 1000 hour
 380 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
55100 psi
@Temperature 302 °F,
Time 1000 hour
 390 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
56600 psi
@Temperature 212 °F,
Time 1000 hour
Tensile Strength, Yield 300 MPa43500 psi
 135 MPa
@Temperature 300 °C
19600 psi
@Temperature 572 °F
 180 MPa
@Temperature 250 °C
26100 psi
@Temperature 482 °F
 240 MPa
@Temperature 200 °C
34800 psi
@Temperature 392 °F
 280 MPa
@Temperature 150 °C
40600 psi
@Temperature 302 °F
 290 MPa
@Temperature 100 °C
42100 psi
@Temperature 212 °F
Elongation at Break 2.5 %2.5 %
Tensile Modulus 90.0 GPa13100 ksi
Fatigue Strength 125 MPa
@Temperature 250 °C
18100 psi
@Temperature 482 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 17.3 µm/m-°C9.61 µin/in-°F
Thermal Conductivity 120 W/m-K833 BTU-in/hr-ft²-°F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 73 %73 %
Iron, Fe 5.0 %5.0 %
Nickel, Ni 2.0 %2.0 %
Silicon, Si 20 %20 %
 
Descriptive Properties
Specific Stiffness33GPa/(g/cc)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RSP Technology RSA-8009 AE Aluminum Super Alloy
RSP Technology RSA-905 AE Aluminum Super Alloy
RSP Technology RSA-443 AE Aluminum Super Alloy
RSP Technology RSA-6061 T6 Aluminum Super Alloy
Aluminum 7075-T6; 7075-T651

NRSP24 / 100838

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.