MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Thermoplastic Polyurethane (TPUR), Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Glass Fiber Reinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Thermoplastic Polyurethane (TPUR), Glass Fiber Reinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.22 - 1.91 g/cc0.0441 - 0.0690 lb/in³Average value: 1.48 g/cc Grade Count:104
Filler Content 5.00 - 76.0 %5.00 - 76.0 %Average value: 32.4 % Grade Count:54
Water Absorption 0.120 - 0.400 %0.120 - 0.400 %Average value: 0.296 % Grade Count:18
Additive Loading 20.0 - 40.0 %20.0 - 40.0 %Average value: 28.3 % Grade Count:6
Maximum Moisture Content 0.05000.0500Average value: 0.0500 Grade Count:3
Linear Mold Shrinkage 0.0000500 - 0.0160 cm/cm0.0000500 - 0.0160 in/inAverage value: 0.00220 cm/cm Grade Count:66
Linear Mold Shrinkage, Transverse 0.000500 - 0.00500 cm/cm0.000500 - 0.00500 in/inAverage value: 0.00188 cm/cm Grade Count:6
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 119 - 125119 - 125Average value: 122 Grade Count:4
Hardness, Shore A 70.0 - 99.070.0 - 99.0Average value: 85.4 Grade Count:11
Hardness, Shore D 50.0 - 75.050.0 - 75.0Average value: 65.4 Grade Count:24
Tensile Strength, Ultimate 14.5 - 1000 MPa2100 - 145000 psiAverage value: 153 MPa Grade Count:99
 30.0 - 65.0 MPa
@Temperature 0.000 - 60.0 °C
4350 - 9430 psi
@Temperature 32.0 - 140 °F
Average value: 43.3 MPa Grade Count:1
 30.0 - 65.0 MPa
@Strain 2.00 - 2.00 %
4350 - 9430 psi
@Strain 2.00 - 2.00 %
Average value: 43.3 MPa Grade Count:1
Tensile Strength, Yield 49.0 - 227 MPa7100 - 32900 psiAverage value: 120 MPa Grade Count:10
Elongation at Break 1.00 - 430 %1.00 - 430 %Average value: 13.9 % Grade Count:96
Elongation at Yield 1.60 - 35.0 %1.60 - 35.0 %Average value: 7.40 % Grade Count:6
Modulus of Elasticity 0.345 - 45.0 GPa50.0 - 6530 ksiAverage value: 9.72 GPa Grade Count:83
Flexural Yield Strength 13.8 - 1150 MPa2000 - 167000 psiAverage value: 259 MPa Grade Count:84
Flexural Modulus 0.234 - 45.0 GPa33.9 - 6530 ksiAverage value: 9.67 GPa Grade Count:87
Compressive Yield Strength 8.27 - 440 MPa1200 - 63800 psiAverage value: 98.9 MPa Grade Count:5
Izod Impact, Notched 0.427 - 5340 J/cm0.800 - 10000 ft-lb/inAverage value: 4.77 J/cm Grade Count:70
 2.00 - 4.00 J/cm
@Temperature -40.0 - -20.0 °C
3.75 - 7.49 ft-lb/in
@Temperature -40.0 - -4.00 °F
Average value: 2.96 J/cm Grade Count:4
Izod Impact, Unnotched 2.14 - 5340 J/cm4.00 - 10000 ft-lb/inAverage value: 12.2 J/cm Grade Count:58
 3.20 - 8.54 J/cm
@Temperature -40.0 - -40.0 °C
5.99 - 16.0 ft-lb/in
@Temperature -40.0 - -40.0 °F
Average value: 5.34 J/cm Grade Count:3
 3.20 - 8.54 J/cm
@Thickness 3.20 - 81.3 mm
5.99 - 16.0 ft-lb/in
@Thickness 0.126 - 3.20 in
Average value: 5.34 J/cm Grade Count:3
Izod Impact, Notched (ISO) 25.0 - 50.4 kJ/m²11.9 - 24.0 ft-lb/in²Average value: 40.1 kJ/m² Grade Count:4
 33.5 - 33.6 kJ/m²
@Temperature -30.0 - -30.0 °C
15.9 - 16.0 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 33.5 kJ/m² Grade Count:2
Charpy Impact Unnotched 10.0 J/cm² - NB47.6 ft-lb/in² - NBAverage value: 15.4 J/cm² Grade Count:12
 6.50 - 16.0 J/cm²
@Temperature -40.0 - -20.0 °C
30.9 - 76.1 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 9.56 J/cm² Grade Count:11
Charpy Impact, Notched 2.73 - 7.14 J/cm²13.0 - 34.0 ft-lb/in²Average value: 4.77 J/cm² Grade Count:24
 0.600 - 3.00 J/cm²
@Temperature -30.0 - -30.0 °C
2.86 - 14.3 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 1.30 J/cm² Grade Count:10
Dart Drop, Total Energy 17.0 - 31.0 J12.5 - 22.9 ft-lbAverage value: 25.7 J Grade Count:3
 14.0 - 25.0 J
@Temperature -29.0 - -29.0 °C
10.3 - 18.4 ft-lb
@Temperature -20.2 - -20.2 °F
Average value: 18.7 J Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+11 - 1.00e+16 ohm-cm1.00e+11 - 1.00e+16 ohm-cmAverage value: 5.56e+14 ohm-cm Grade Count:18
Dielectric Constant 3.60 - 4.903.60 - 4.90Average value: 4.33 Grade Count:7
Dielectric Strength 14.2 - 19.7 kV/mm360 - 500 kV/inAverage value: 17.0 kV/mm Grade Count:7
Dissipation Factor 0.00300 - 0.02000.00300 - 0.0200Average value: 0.0136 Grade Count:7
 
Thermal PropertiesMetricEnglishComments
CTE, linear 9.00 - 162 µm/m-°C5.00 - 90.0 µin/in-°FAverage value: 47.8 µm/m-°C Grade Count:22
Thermal Conductivity 0.231 - 0.403 W/m-K1.60 - 2.80 BTU-in/hr-ft²-°FAverage value: 0.323 W/m-K Grade Count:5
Melting Point 190 °C374 °FAverage value: 190 °C Grade Count:3
Maximum Service Temperature, Air 80.0 - 90.0 °C176 - 194 °FAverage value: 87.5 °C Grade Count:4
Deflection Temperature at 0.46 MPa (66 psi) 83.3 - 170 °C182 - 338 °FAverage value: 127 °C Grade Count:25
Deflection Temperature at 1.8 MPa (264 psi) 54.4 - 185 °C130 - 365 °FAverage value: 101 °C Grade Count:58
Vicat Softening Point 87.0 - 186 °C189 - 367 °FAverage value: 137 °C Grade Count:10
Minimum Service Temperature, Air -30.0 °C-22.0 °FAverage value: -30.0 °C Grade Count:3
Flammability, UL94 HB - V-0HB - V-0Grade Count:38
 
Processing PropertiesMetricEnglishComments
Processing Temperature 70.0 - 265 °C158 - 509 °FAverage value: 194 °C Grade Count:46
Nozzle Temperature 221 - 260 °C430 - 500 °FAverage value: 242 °C Grade Count:11
Die Temperature 245 - 260 °C473 - 500 °FAverage value: 253 °C Grade Count:5
Melt Temperature 188 - 265 °C370 - 509 °FAverage value: 239 °C Grade Count:47
Mold Temperature 20.0 - 121 °C68.0 - 250 °FAverage value: 68.5 °C Grade Count:77
Injection Velocity 50.8 - 76.2 mm/sec2.00 - 3.00 in/secAverage value: 63.5 mm/sec Grade Count:5
Drying Temperature 70.0 - 132 °C158 - 270 °FAverage value: 98.8 °C Grade Count:47
Moisture Content 0.0100 - 0.0500 %0.0100 - 0.0500 %Average value: 0.0200 % Grade Count:33
Dew Point -40.0 - -28.9 °C-40.0 - -20.0 °FAverage value: -38.6 °C Grade Count:24
Injection Pressure 4.96 - 103 MPa720 - 15000 psiAverage value: 83.0 MPa Grade Count:51
Cushion 0.635 cm0.250 inAverage value: 0.635 cm Grade Count:5

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Silicone Polyurethane, Ether Based
Overview of materials for Thermoplastic Polyurethane (TPUR), Polyester Grade
Overview of materials for Thermoplastic Polyurethane, Elastomer, Ether Grade
Overview of materials for Thermoplastic Polyurethane, Elastomer, Glass Filled
Overview of materials for Thermoset Polyurethane, Elastomer, Unreinforced

O5046 / 78465

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.