Arkema Orgalloy® RS 6000 NAT Polyamide 6 Alloy
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, Unreinforced
Material Notes:
Polyamide Alloy, Rigid grade, Nylon 6 based
Tubes / Mandrels / Profiles / Cables
Information provided by Arkema Group
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.03
g/cc
0.0372
lb/in³
ISO 1183
1.03
g/cc
0.0372
lb/in³
Cond.; ISO 1183
Water Absorption
3.3 %
3.3 %
Dry; Sim. to ISO 62
Moisture Absorption
1.30 %
1.30 %
Dry; Sim. to ISO 62
Linear Mold Shrinkage, Flow
0.0070
cm/cm
0.0070
in/in
Dry; ISO 294-4, 2577
0.0090
cm/cm
0.0090
in/in
Melt Flow
8.0
g/10 min
@Load 2.16 kg,
Temperature 235 °C
8.0
g/10 min
@Load 4.76 lb,
Temperature 455 °F
cm³/10 min Volumetric Rate; ISO 1133
Mechanical Properties
Metric
English
Comments
Hardness, Shore D
73
@Time 15.0 sec
73
@Time 0.00417 hour
Dry; ISO 7619-1
Tensile Strength, Yield
48.0
MPa
6960
psi
Cond.; ISO 527-1/-2
55.0
MPa
7980
psi
Dry; ISO 527-1/-2
Elongation at Break
15 %
15 %
Dry; ISO 527-1/-2
>= 50 %
>= 50 %
Cond.; ISO 527-1/-2
Elongation at Yield
4.0 %
4.0 %
Dry; ISO 527-1/-2
6.0 %
6.0 %
Cond.; ISO 527-1/-2
Tensile Modulus
1.95
GPa
283
ksi
Cond.; ISO 527-1/-2
2.23
GPa
323
ksi
Dry; ISO 527-1/-2
Charpy Impact Unnotched
NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Cond.; ISO 179/1eU
Charpy Impact, Notched
0.500
J/cm²
@Temperature 23.0 °C
2.38
ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
0.900
J/cm²
@Temperature 23.0 °C
4.28
ft-lb/in²
@Temperature 73.4 °F
Cond.; ISO 179/1eA
Tensile Creep Modulus, 1 hour
2030
MPa
294000
psi
Cond.; ISO 899-1
Tensile Creep Modulus, 1000 hours
870
MPa
126000
psi
Cond.; ISO 899-1
Electrical Properties
Metric
English
Comments
Volume Resistivity
>=
1.00e+15
ohm-cm
>=
1.00e+15
ohm-cm
Surface Resistance
>=
1.00e+15
ohm
>=
1.00e+15
ohm
Cond.; IEC 60093
Dielectric Constant
3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
Cond; IEC 60250
3.0
@Frequency 100 Hz
3.0
@Frequency 100 Hz
Cond.; IEC 60250
Dielectric Strength
38.0
kV/mm
965
kV/in
Dry; IEC 60243-1
38.0
kV/mm
965
kV/in
Cond.; IEC 60243-1
Dissipation Factor
0.025
@Frequency 1e+6 Hz
0.025
@Frequency 1e+6 Hz
Cond.; 0
0.062
@Frequency 100 Hz
0.062
@Frequency 100 Hz
Cond.; IEC 60250
Comparative Tracking Index
600
V
600
V
Cond.; IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
93.0
µm/m-°C
51.7
µin/in-°F
Dry; ISO 11359-1/-2
CTE, linear, Transverse to Flow
133
µm/m-°C
73.9
µin/in-°F
Dry; ISO 11359-1/-2
Melting Point
220
°C
428
°F
10°C/min; Dry; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi)
130
°C
266
°F
Dry; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi)
54.0
°C
129
°F
Dry; ISO 75-1/-2
Vicat Softening Point
150
°C
302
°F
50°C/h 50N; Dry; ISO 306
Flammability, UL94
HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
IEC 60695-11-10
HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
IEC 60695-11-10
Processing Properties
Metric
English
Comments
Melt Temperature
260
°C
500
°F
Injection Molding; ISO 294
Mold Temperature
60.0
°C
140
°F
Injection Molding; ISO 10724
Descriptive Properties
Form as Delivered
Pellets
Heat Stabilized
Yes
Light Stabilized
Yes
Moisture Sensitive
Yes
Processing Methods
Injection Molding
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Arkema Orgalloy® LE 6000 NAT Polyamide 6 Alloy
Arkema Orgalloy® LE 60 LM XV NAT Polyamide 6 Alloy
Arkema Orgalloy® RS 6600 BLACK Polyamide 6.6 Alloy
Arkema ORGASOL® 1002 D Nat 1 Polyamide 6
A. Schulman ComAlloy Hiloy® 612 Nylon 6, Glass Reinforced, UL
PARKG445 / 24500
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.