MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Aluminum 2618-T61
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92618; Aluminium 2618-T61; AA2618-T61; Al2618-T61
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.76 g/cc0.0997 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 115115AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 144144Converted from Brinell Hardness Value
Hardness, Rockwell A 45.545.5Converted from Brinell Hardness Value
Hardness, Rockwell B 7272Converted from Brinell Hardness Value
Hardness, Vickers 130130Converted from Brinell Hardness Value
Tensile Strength, Ultimate 441 MPa64000 psiAA; Typical
 34.0 MPa
@Temperature 371 °C
4930 psi
@Temperature 700 °F
 52.0 MPa
@Temperature 316 °C
7540 psi
@Temperature 601 °F
 90.0 MPa
@Temperature 260 °C
13100 psi
@Temperature 500 °F
 221 MPa
@Temperature 204 °C
32100 psi
@Temperature 399 °F
 345 MPa
@Temperature 149 °C
50000 psi
@Temperature 300 °F
 427 MPa
@Temperature 100 °C
61900 psi
@Temperature 212 °F
 441 MPa
@Temperature -28.0 °C
64000 psi
@Temperature -18.4 °F
 441 MPa
@Temperature 24.0 °C
64000 psi
@Temperature 75.2 °F
 462 MPa
@Temperature -80.0 °C
67000 psi
@Temperature -112 °F
 538 MPa
@Temperature -196 °C
78000 psi
@Temperature -321 °F
 350 MPa
@Thickness 76.23 - 102 mm
50800 psi
@Thickness 3.001 - 4.00 in
Hand forgings; Short transverse
 360 MPa
@Thickness <=50.8 mm
52200 psi
@Thickness <=2.00 in
Hand forgings; Short transverse
 360 MPa
@Thickness 50.83 - 76.2 mm
52200 psi
@Thickness 2.001 - 3.00 in
Hand forgings; Short transverse
 365 MPa
@Thickness 76.23 - 102 mm
52900 psi
@Thickness 3.001 - 4.00 in
Hand forgings; Long transverse
 380 MPa
@Thickness <=102 mm
55100 psi
@Thickness <=4.00 in
Die forgings; Axis not parallel to grain flow
 380 MPa
@Thickness <=50.8 mm
55100 psi
@Thickness <=2.00 in
Hand forgings; Long transverse
 380 MPa
@Thickness 50.83 - 76.2 mm
55100 psi
@Thickness 2.001 - 3.00 in
Hand forgings; Long transverse
 380 MPa
@Thickness <=63.5 mm
55100 psi
@Thickness <=2.50 in
Rolled rings; Tangential
 380 MPa
@Thickness <=63.5 mm
55100 psi
@Thickness <=2.50 in
Rolled rings; Axial
 385 MPa
@Thickness 76.23 - 102 mm
55800 psi
@Thickness 3.001 - 4.00 in
Hand forgings; Longitudinal
 395 MPa
@Thickness 50.83 - 76.2 mm
57300 psi
@Thickness 2.001 - 3.00 in
Hand forgings; Longitudinal
 400 MPa
@Thickness <=102 mm
58000 psi
@Thickness <=4.00 in
Die forgings; Axis parallel to grain flow
 400 MPa
@Thickness <=50.8 mm
58000 psi
@Thickness <=2.00 in
Hand forgings; Longitudinal
Tensile Strength, Yield 372 MPa54000 psiAA; Typical
 270 MPa
@Thickness 76.23 - 102 mm
39200 psi
@Thickness 3.001 - 4.00 in
Hand forgings; Short transverse
 275 MPa
@Thickness 76.23 - 102 mm
39900 psi
@Thickness 3.001 - 4.00 in
Hand forgings; Long transverse
 285 MPa
@Thickness <=63.5 mm
41300 psi
@Thickness <=2.50 in
Rolled rings; Tangential
 285 MPa
@Thickness <=63.5 mm
41300 psi
@Thickness <=2.50 in
Rolled rings; Axial
 290 MPa
@Thickness <=102 mm
42100 psi
@Thickness <=4.00 in
Die forgings; Axis not parallel to grain flow
 290 MPa
@Thickness <=50.8 mm
42100 psi
@Thickness <=2.00 in
Hand forgings; Long transverse
 290 MPa
@Thickness <=50.8 mm
42100 psi
@Thickness <=2.00 in
Hand forgings; Short transverse
 290 MPa
@Thickness 50.83 - 76.2 mm
42100 psi
@Thickness 2.001 - 3.00 in
Hand forgings; Long transverse
 290 MPa
@Thickness 50.83 - 76.2 mm
42100 psi
@Thickness 2.001 - 3.00 in
Hand forgings; Short transverse
 310 MPa
@Thickness <=102 mm
45000 psi
@Thickness <=4.00 in
Die forgings; Axis parallel to grain flow
 310 MPa
@Thickness 76.23 - 102 mm
45000 psi
@Thickness 3.001 - 4.00 in
Hand forgings; Longitudinal
 315 MPa
@Thickness 50.83 - 76.2 mm
45700 psi
@Thickness 2.001 - 3.00 in
Hand forgings; Longitudinal
 325 MPa
@Thickness <=50.8 mm
47100 psi
@Thickness <=2.00 in
Hand forgings; Longitudinal
 24.0 MPa
@Strain 0.2 %,
Temperature 371 °C
3480 psi
@Strain 0.2 %,
Temperature 700 °F
 31.0 MPa
@Strain 0.2 %,
Temperature 316 °C
4500 psi
@Strain 0.2 %,
Temperature 601 °F
 62.0 MPa
@Strain 0.2 %,
Temperature 260 °C
8990 psi
@Strain 0.2 %,
Temperature 500 °F
 179 MPa
@Strain 0.2 %,
Temperature 204 °C
26000 psi
@Strain 0.2 %,
Temperature 399 °F
 303 MPa
@Strain 0.2 %,
Temperature 149 °C
43900 psi
@Strain 0.2 %,
Temperature 300 °F
 372 MPa
@Strain 0.2 %,
Temperature -28.0 °C
54000 psi
@Strain 0.2 %,
Temperature -18.4 °F
 372 MPa
@Strain 0.2 %,
Temperature 24.0 °C
54000 psi
@Strain 0.2 %,
Temperature 75.2 °F
 372 MPa
@Strain 0.2 %,
Temperature 100 °C
54000 psi
@Strain 0.2 %,
Temperature 212 °F
 379 MPa
@Strain 0.2 %,
Temperature -80.0 °C
55000 psi
@Strain 0.2 %,
Temperature -112 °F
 421 MPa
@Strain 0.2 %,
Temperature -196 °C
61100 psi
@Strain 0.2 %,
Temperature -321 °F
Elongation at Break  10 %
@Temperature -28.0 °C
10 %
@Temperature -18.4 °F
 10 %
@Temperature 24.0 °C
10 %
@Temperature 75.2 °F
 10 %
@Temperature 100 °C
10 %
@Temperature 212 °F
 11 %
@Temperature -80.0 °C
11 %
@Temperature -112 °F
 12 %
@Temperature -196 °C
12 %
@Temperature -321 °F
 14 %
@Temperature 149 °C
14 %
@Temperature 300 °F
 24 %
@Temperature 204 °C
24 %
@Temperature 399 °F
 50 %
@Temperature 260 °C
50 %
@Temperature 500 °F
 80 %
@Temperature 316 °C
80 %
@Temperature 601 °F
 120 %
@Temperature 371 °C
120 %
@Temperature 700 °F
 4.0 %
@Thickness <=102 mm
4.0 %
@Thickness <=4.00 in
Die forgings; Axis parallel to grain flow
 4.0 %
@Thickness <=102 mm
4.0 %
@Thickness <=4.00 in
Die forgings; Axis not parallel to grain flow
 4.0 %
@Thickness <=50.8 mm
4.0 %
@Thickness <=2.00 in
Hand forgings; Short transverse
 4.0 %
@Thickness 50.83 - 76.2 mm
4.0 %
@Thickness 2.001 - 3.00 in
Hand forgings; Short transverse
 4.0 %
@Thickness 76.23 - 102 mm
4.0 %
@Thickness 3.001 - 4.00 in
Hand forgings; Short transverse
 5.0 %
@Thickness <=50.8 mm
5.0 %
@Thickness <=2.00 in
Hand forgings; Long transverse
 5.0 %
@Thickness 50.83 - 76.2 mm
5.0 %
@Thickness 2.001 - 3.00 in
Hand forgings; Long transverse
 5.0 %
@Thickness 76.23 - 102 mm
5.0 %
@Thickness 3.001 - 4.00 in
Hand forgings; Long transverse
 5.0 %
@Thickness <=63.5 mm
5.0 %
@Thickness <=2.50 in
Rolled rings; Axial
 6.0 %
@Thickness <=63.5 mm
6.0 %
@Thickness <=2.50 in
Rolled rings; Tangential
 7.0 %
@Thickness <=50.8 mm
7.0 %
@Thickness <=2.00 in
Hand forgings; Longitudinal
 7.0 %
@Thickness 50.83 - 76.2 mm
7.0 %
@Thickness 2.001 - 3.00 in
Hand forgings; Longitudinal
 7.0 %
@Thickness 76.23 - 102 mm
7.0 %
@Thickness 3.001 - 4.00 in
Hand forgings; Longitudinal
 10 %
@Diameter 12.7 mm
10 %
@Diameter 0.500 in
AA; Typical
Modulus of Elasticity 74.5 GPa10800 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Compressive Strength 370 MPa53700 psi
Poissons Ratio 0.330.33
Fatigue Strength 124 MPa
@# of Cycles 5.00e+8
18000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPa3920 ksiCalculated
Shear Strength 262 MPa38000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000470 ohm-cm0.00000470 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  20.6 µm/m-°C
@Temperature -50.0 - 20.0 °C
11.4 µin/in-°F
@Temperature -58.0 - 68.0 °F
 22.3 µm/m-°C
@Temperature 20.0 - 100 °C
12.4 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 23.2 µm/m-°C
@Temperature 20.0 - 200 °C
12.9 µin/in-°F
@Temperature 68.0 - 392 °F
 24.0 µm/m-°C
@Temperature 20.0 - 300 °C
13.3 µin/in-°F
@Temperature 68.0 - 572 °F
average
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
13.4 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.875 J/g-°C0.209 BTU/lb-°F
Thermal Conductivity 146 W/m-K1010 BTU-in/hr-ft²-°F
Melting Point 549 - 638 °C1020 - 1180 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 549 °C1020 °FAA; Typical
Liquidus 638 °C1180 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Solution Temperature 529 °C985 °F
Aging Temperature 199 °C390 °Ffor 20 hr at temperature
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 92.4 - 94.9 %92.4 - 94.9 %As remainder
Copper, Cu 1.9 - 2.7 %1.9 - 2.7 %
Iron, Fe 0.90 - 1.3 %0.90 - 1.3 %
Magnesium, Mg 1.3 - 1.8 %1.3 - 1.8 %
Nickel, Ni 0.90 - 1.2 %0.90 - 1.2 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 0.10 - 0.25 %0.10 - 0.25 %
Titanium, Ti 0.04 - 0.10 %0.04 - 0.10 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 2618-T6
Aluminum 2618-T61 (Includes Creep/Rupture Data)
Aluminum 7075-T6; 7075-T651
Aluminum 6061-T6; 6061-T651
Alclad Aluminum 7075-T6, T651

MA2618T61 / 8971

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.