MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Saint-Gobain Tygon® A-60-F I.B. Pressure Tubing Formulation for CIP and SIP cleaning and sterilization systems
Categories: Polymer; Thermoplastic

Material Notes: Good for use in clean-in-place and steam-in-place cleaning and sterilization systems, Norprene® Pressure Tubing has excellent alkali resistance and is compatible with numerous oxidizing agents such as hydrogen peroxide, sodium hypochlorite and ozone.

Norprene® Pressure Tubing fully complies with FDA 177.2600 criteria, 3A Sanitary Standards and NSF Standard 51, which are applicable to many food contact applications.

Norprene® Pressure Tubing exhibits excellent resistance to ozone and UV light, with little or no signs of deterioration in laboratory testing equivalent to 10 years of outdoor exposure. Norprene® Pressure Tubing provides long service life when exposed to heat, abrasion and pressure. It is temperature resistant up to 275°F and retains flexibility to -60°F.

Features and Benefits

  • Handles at least 4 times the pressure of non-reinforced tubing
  • Temperature resistant from -60°F to 275°F
  • Ozone and UV light resistant
  • Repeatedly autoclavable
  • Chemically compatible with a wide range of fluids
  • Meets FDA, 3A and NSF Criteria

Information provided by Saint Gobain Performance Products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.980 g/ccASTM D792-00
Water Absorption 0.30 %
@Temperature 22.8 °C,
Time 86400 sec
ASTM D570-98
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 61
@Time 15.0 sec
ASTM D2240-03
Tensile Strength 1000 psiASTM D412-98
Elongation at Break 375 %ASTM D412-98
100% Modulus 0.410 ksi
@Strain 100 %
ASTM D412-98
300% Modulus 0.800 ksi
@Strain 300 %
ASTM D412-98
Tear Strength 120 pliASTM D1004-03
Compression Set 30 %
@Temperature 70.0 °C,
Time 79200 sec
ASTM D395-03 Method B
Tensile Set 47 %at 75% Elongation; ASTM D412-98
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 535 V/milASTM D149-97
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 275 °F
Brittleness Temperature -75.0 °FASTM D746-98
 
Compliance PropertiesOriginal ValueComments
FDA Yes
NSF Yes
 
Descriptive Properties
ColorCream

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Saint-Gobain Tygon® A-60-F Food Process Tubing Formulation
Saint-Gobain Tygon® A-60-G Industrial Grade Tubing Formulation
Saint-Gobain Tygon® Noroprene® Chemical Tubing Formulation
Saint-Gobain Tygon® A-60-N Drinking Water Tubing Formulation
Saint-Gobain Norton® Tygon® 2075 Ultra Chemical Resistant Tubing Formulation

PSTGQ903 / 160399

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.