MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Saint-Gobain Norton® PFA Fluoropolymer Film
Categories: Polymer; Film; Thermoplastic; Fluoropolymer; Perfluoroalkoxy (PFA)

Material Notes: Features/Benefits:
  • Outstanding flex life and stress crack resistance
  • Performance from -254°C (-425°F) to 260°C (500°F)
  • Outstanding anti-stick release properties
  • Excellent electrical properties
  • Excellent weatherability
  • Product thicknesses from 0.0005" (0.0127 mm) to 0.030" (0.76 mm)
  • Width up to 62" (1575 mm) for 0.0005" to 0.010" and up to 48" for over 0.010"
  • All films are manufactured and converted in class 100,000 clean room facility
  • Available in cementable (surface treated) form

Norton® PFA fluoropolymer film is manufactured by Saint-Gobain Advanced Films and Fabrics from perfluoroalkoxy (PFA) polymer resin. This film offers the highest continuous use temperature 260°C (500°F) of any melt-processable fluoropolymer film. Norton PFA film offers many of the performance properties of PTFE in a clear, transparent form and can be heat sealed, thermoformed, welded, metallized, or laminated to a wide variety of materials.

Norton® PFA film offers a combination of excellent dielectric properties across a wide temperature and frequency range, the highest level of chemical and stress crack resistance, excellent clarity and weatherability. The chemical resistance of PFA provides excellent tank-lining performance.

Norton® PFA Type WF (mechanical grade) is an ideal economical solution for applications that don't require high aesthetic standards, such as hot melt adhesive (welding tape) application. PFA WF grade possesses all physical, mechanical, and thermal properties of PFA film while offering up to 25% savings.

Surface Treatments Available: C-Treatable (cementable, 1 or 2 sides); Corona Treatment (1 or 2 sides); Chemical Etching (1 or 2 sides)
Flammability (UL-94): V-0

The combination of chemical resistance and high temperature resistance over a wide frequency range make Norton PFA film an ideal component for circuit board fabricators, flat cable, and electrical insulation applications. Product thickness availability from 0.0005" through 0.030" at widths up to 62" offers circuit board designers flexibility in structure design.

The high temperature resistance and non-wetting surface of Norton PFA make it an ideal material for use as a high temperature release film or bagging film for composite manufacturers. The continuous use temperature of 260°C (500°F) and a melt point 310°C (590°F) meet the needs of new resin systems requiring a 230°C (446°F) cure temperature.

Specification Notes: All values represent typical performance properties and should not be used for specification purposes.
Information provided by Saint Gobain Performance Products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.12 - 2.18 g/ccASTM D-792
Water Absorption <= 0.010 %
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 2250 psiASTM D-882
Elongation at Break 300 %ASTM D-882
Tensile Modulus 70000 psiASTM D-882
Tear Strength 100 kg(f)/cmInitial Tear Strength; ASTM D-1004
Elmendorf Tear Strength, MD 125 - 135 g/mil(direction not reported), Propagation Tear Strength; ASTM D-1922
 
Electrical PropertiesOriginal ValueComments
Surface Resistivity per Square 1.00e+15 ohmASTM D-257
Dielectric Constant 2.1
@Frequency 1000 Hz
ASTM D-150
Dielectric Strength 4700 V/milValue for a 1 mil sample.; ASTM D-149
Dissipation Factor 0.00050
@Frequency 1000 Hz
ASTM D-150
 
Thermal PropertiesOriginal ValueComments
CTE, linear 55.0 µin/in-°F
@Temperature 20.0 °C
ASTM D-696
Specific Heat Capacity 0.280 BTU/lb-°F
Thermal Conductivity 1.35 BTU-in/hr-ft²-°FASTM D-2863
Melting Point 575 - 590 °FASTM D-3418
Maximum Service Temperature, Air 500 °FUL-746 B
Flammability, UL94 V-0
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.35ASTM D542
Transmission, Visible 96 %ASTM E424
 
Descriptive Properties
Fold Endurance (MIT)600000, MinASTM D-2176

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Saint-Gobain Norton® PVDF Fluoropolymer Film
Saint-Gobain Norton® FEP Fluoropolymer Film
Saint-Gobain Norton® Fluorglas® Chemfilm® R191 Skived Sintered PTFE Tape (0.003" thick)
Saint-Gobain Norton® MFA Fluoropolymer Film
Arkema Kynar® 710 Polyvinylidene Fluoride Homopolymer- Injection Molding

PSTGQZ156 / 68670

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.