MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Zenite® 7140X BK010 LCP
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), 40% Glass Fiber Filled

Material Notes: Zenite® 7140X BK010 is a 40% glass reinforced liquid crystal polymer resin with improved weldline strength, low post soldering warpage and a heat deflection temperature of 298ºC.

Celenese acquired the Zenite product line from DuPont in 2010.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.77 g/ccISO 1183
Filler Content 40 %
Linear Mold Shrinkage, Flow 0.0020 cm/cm
@Thickness 2.00 mm
ISO 294-4
Linear Mold Shrinkage, Transverse 0.0070 cm/cm
@Thickness 2.00 mm
ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 120 MPaISO 527
Elongation at Break 1.5 %ISO 527
Tensile Modulus 16500 MPaISO 527
Flexural Strength 170 MPa
@Temperature 23.0 °C
ISO 178
Flexural Modulus 14000 MPa
@Temperature 23.0 °C
ISO 178
Charpy Impact, Notched 1.00 J/cm²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 175 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 352 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 298 °CISO 75-1/-2 1993/N2
Flammability, UL94 V-0
@Thickness 0.750 mm
IEC 60695-11-10
 V-0
@Thickness 0.400 mm
IEC 60695-11-10
 V-0
@Thickness 0.750 mm
UL94
 V-0
@Thickness 0.400 mm
UL94
 
Processing PropertiesOriginal ValueComments
Melt Temperature 365 °COptimum
 360 - 370 °C
Mold Temperature 80.0 °COptimum
 40.0 - 150 °C
Drying Temperature 150 °C
Dry Time 3 hourDehumidified Dryer
Moisture Content <= 0.010 %
 
Descriptive Properties
ColorBlack
Drying RecommendedYes
FillerGlass Reinforced
FormsPellets
GenericLCP
Part Marking Code>LCP-GF40<ISO 11469
Polymer FamilyLCP
Polymer TypeLCP
Processing MethodInjection Molding
Product CategoryGlass Reinforced Resins
Region AvailableAmericas
 Asia/Pacific
 Europe
Resin IdentificationLCP-GF40ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Zenite® 9140HT NC010 LCP
Celanese VECTRA T.rex541 LCP, 40% Specialty
Overview of materials for Liquid Crystal Polymer (LCP), 40% Glass Fiber Filled
Avient Stat-Tech™ LC-40CF/000 Natural LCP (Liquid Crystal Polymer), 40% Carbon Fiber Reinforced, Electrically Conductive, EMI/RFI Shielding
Celanese VECTRA E463i LCP, 40% Mineral / Glass Reinforced

PDTA7785 / 89628

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.