MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 3003-H14
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 3000 Series Aluminum Alloy

Material Notes: Good weldability/formability and very good corrosion resistance lead to applications such as food and chemical handling, tanks, trim, litho sheet, pressure vessels, and piping.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A93003; ISO AlMn1Cu; Aluminium 3003-H14; AA3003-H14; Al3003-H14
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.73 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 40AA; Typical; 500 g load; 10 mm ball
Tensile Strength, Ultimate 22.0 ksiAA; Typical
 18.0 MPa
@Temperature 400 °C
 29.0 MPa
@Temperature 300 °C
 96.0 MPa
@Temperature 200 °C
 145 MPa
@Temperature 100 °C
 150 MPa
@Temperature -30.0 °C
 150 MPa
@Temperature 25.0 °C
 175 MPa
@Temperature -100 °C
 250 MPa
@Temperature -200 °C
 140 - 180 MPa
@Thickness 0.229 - 25.4 mm
Tensile Strength, Yield 21.0 ksiAA; Typical
 12.0 MPa
@Temperature 400 °C
 17.0 MPa
@Temperature 300 °C
 62.0 MPa
@Temperature 200 °C
 130 MPa
@Temperature 100 °C
 145 MPa
@Temperature -30.0 °C
 145 MPa
@Temperature 25.0 °C
 155 MPa
@Temperature -100 °C
 170 MPa
@Temperature -200 °C
 >= 115 MPa
@Thickness 0.229 - 25.4 mm
Elongation at Break 16 %
@Temperature -30.0 °C
 16 %
@Temperature 25.0 °C
 16 %
@Temperature 100 °C
 19 %
@Temperature -100 °C
 20 %
@Temperature 200 °C
 30 %
@Temperature -200 °C
 70 %
@Temperature 300 °C
 75 %
@Temperature 400 °C
 1.0 - 10 %
@Thickness 0.229 - 25.4 mm
 8.0 %
@Thickness 1.59 mm
AA; Typical
 16 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Notched Tensile Strength 172 MPa2.5 cm width x 0.16 cm thick side-notched specimen, Kt = 17.
Ultimate Bearing Strength 241 MPaEdge distance/pin diameter = 2.0
Bearing Yield Strength 193 MPaEdge distance/pin diameter = 2.0
Poissons Ratio 0.33
Fatigue Strength 9000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 30 %0-100 Scale of Aluminum Alloys
Shear Modulus 25.0 GPa
Shear Strength 14.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 25.0 ohm-cir-mil/ft
@Temperature 20.0 °C
AA; Typical
Magnetic Susceptibility 8.0e-7cgs/g at 25ºC
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.9 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 21.5 µm/m-°C
@Temperature -50.0 - 20.0 °C
 24.1 µm/m-°C
@Temperature 20.0 - 200 °C
 25.1 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.893 J/g-°C
Thermal Conductivity 1100 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 1190 - 1210 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 1190 °FAA; Typical
Liquidus 1210 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °FCommercial practice: 750 to 1100°F, higher temperatures used only for flash annealing.
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 96.7 - 99 %As remainder
Copper, Cu 0.05 - 0.20 %
Iron, Fe <= 0.70 %
Manganese, Mn 1.0 - 1.5 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.60 %
Zinc, Zn <= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 3003-H12
Aluminum 3003-O
Aluminum 5052-H32
Aluminum 3003-H16

MA3003H14 / 8981

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.