MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Sumitomo Bakelite North America RX® 655 Novolac Phenolic
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Phenolic; Phenolic, Novolac, Mineral/Glass Filled

Material Notes: Fiberglass and mineral reinforced phenolic molding compound with very high fill level (75%). Excellent dimensional stability and good strength at elevated temperatures. Very low thermal expansion coefficient and negligible creep under load.

Information provided by Vyncolit, a Sumitomo Bakelite Group

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.950 g/cc0.0343 lb/in³Powder Density; ISO 60
Density 2.10 g/cc0.0759 lb/in³Relative Density; ISO 1183
Linear Mold Shrinkage 0.00060 cm/cm0.00060 in/inCompression Molding; ISO 2577
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell E 105105ISO 2039/2
Tensile Strength at Break 100 MPa14500 psiISO 527
Flexural Strength 165 MPa23900 psiAt Rupture; ISO 178
Flexural Modulus 27.0 GPa3920 ksiISO 178
Compressive Strength 410 MPa59500 psiISO 604
Charpy Impact, Notched 0.200 J/cm²0.952 ft-lb/in²ISO 179
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 14.0 kV/mm
@Thickness 3.00 mm
356 kV/in
@Thickness 0.118 in
ASTM D149
Arc Resistance 180 sec180 secASTM D495
Comparative Tracking Index 250 V250 VIEC 112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 17.0 µm/m-°C
@Temperature 20.0 °C
9.44 µin/in-°F
@Temperature 68.0 °F
TMA
Thermal Conductivity 0.940 W/m-K6.52 BTU-in/hr-ft²-°FASTM C-518
Deflection Temperature at 1.8 MPa (264 psi) 200 °C392 °FAs molded; ISO 75 A
 >= 282 °C>= 540 °FPost Baked; ISO 75 A
 
Descriptive Properties
ColorBlack
FormGranular
Main FillerGlass Fiber & Mineral
Molding MethodCompression, transfer, injection

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Plenco 6401 Phenolic, Briquette, Injection Molded
Vyncolit X655 Novolac Phenolic
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Aluminum 6061-T6; 6061-T651
Plenco 6401 Phenolic, Granular, Compression Molded

PVYNC017 / 72225

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.