MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Moplen EP548U Polypropylene, Impact Modified; Molded/Extruded
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Impact Modified; Molded/Extruded

Material Notes: Moplen EP548U is a nucleated heterophasic copolymer with antistatic activation, used in injection molding applications. It exhibits an good impact/stiffness balance combined with a high fluidity. Moplen EP548U is typically used in opaque containers, house wares, toys and in thin-walled containers for food packaging (e.g. margarine tubs, yoghurt pots, etc.). Applications: House wares, Opaque Containers, Sports, Leisure & Toys

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ISO 1183-1
Melt Flow 70 g/10 min
@Load 2.16 kg,
Temperature 230 °C
70 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133-1
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 28.0 MPa4060 psiISO 527-1,-2
Elongation at Break >= 30 %>= 30 %ISO 527-1,-2
Elongation at Yield 5.0 %5.0 %ISO 527-1,-2
Tensile Modulus 1.45 GPa210 ksiISO 527-1,-2
Charpy Impact, Notched  0.300 J/cm²
@Temperature -20.0 °C
1.43 ft-lb/in²
@Temperature -4.00 °F
Type 1, Edgewise, Notch A; ISO 179
 0.350 J/cm²
@Temperature 0.000 °C
1.67 ft-lb/in²
@Temperature 32.0 °F
Type 1, Edgewise, Notch A; ISO 179
 0.400 J/cm²
@Temperature 23.0 °C
1.90 ft-lb/in²
@Temperature 73.4 °F
Type 1, Edgewise, Notch A; ISO 179
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 95.0 °C203 °Funannealed; ISO 75B-1,-2
Vicat Softening Point 151 °C304 °FA50; ISO 306
Brittleness Temperature -53.0 °C-63.4 °FISO 6603-2
 
Descriptive Properties
Processing MethodInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Moplen EP548P Polypropylene, Impact Modified; Molded/Extruded
LyondellBasell Moplen EP548Q Polypropylene, Impact Modified; Molded/Extruded
LyondellBasell Moplen EP548L Polypropylene, Impact Modified; Molded/Extruded
LyondellBasell Moplen EP548S Polypropylene, Impact Modified; Molded/Extruded
LyondellBasell Moplen EP548R Polypropylene, Impact Modified; Molded/Extruded

PEQT8965 / 220599

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.