MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Teijin Films Melinex® 606 Polyester Film, 300 Gauge
Categories: Polymer; Film; Thermoplastic; Polyester, TP; Polyester Film

Material Notes: Melinex® 606 is a very smooth two-side coated polyester film designed specifically for high density floppy disks.

Also available in 285 Gauge

Information provided by DuPont.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.395 g/ccASTM D1505
Thickness 3.00 mil
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 13900 psi
@Strain >=5 %
ASTM D882A
Film Tensile Strength at Yield, TD 13900 psi
@Strain >=5 %
ASTM D882A
Secant Modulus, MD 492 ksiASTM D882A
Secant Modulus, TD 610 ksiASTM D882A
Film Tensile Strength at Break, MD 27700 psiASTM D882A
Film Tensile Strength at Break, TD 32600 psiASTM D882A
 
Thermal PropertiesOriginal ValueComments
Shrinkage, MD 2.5 %
@Temperature 190 °C,
Time 300 sec
Unrestrained
Shrinkage, TD 1.0 %
@Temperature 190 °C,
Time 300 sec
Unrestrained
 
Optical PropertiesOriginal ValueComments
Transmission, Visible 90.2 %TLT; ASTM D1003
 
Descriptive Properties
Coefficient of Hygroscopic Expansion7E-06per 40% - 80% RH

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Teijin Films Melinex® 694 Polyester Film
DuPont Teijin Films Melinex® 542 Polyester Film
DuPont Teijin Films Melinex® 617 Polyester Film, 500 Gauge
DuPont Teijin Films Melinex® 583 Polyester Film, 300 Gauge
DuPont Teijin Films Melinex® 581 Polyester Film

PDTZ9176 / 139519

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.