MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Ineos ABS Lustran® ABS 595CP Refrigeration and Extrusion Grade  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Extruded

Material Notes: Lustran® ABS 595CP is refrigeration and extrusion grade, resistant to cyclopentane, and has high impact strength.

Lustran® is now a product of INEOS Styrolution. Information provided by the manufacturer.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
Melt Flow 3.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 112ISO 2039-2
Tensile Strength at Break 38.0 MPa50 mm/min; ISO 527-1,-2
Tensile Strength, Yield 46.0 MPa50 mm/min; ISO 527-1,-2
Elongation at Break >= 25 %50 mm/min; acc. ISO 527-1,-2
Tensile Modulus 2.55 GPa1 mm/min; ISO 527-1,-2
Flexural Strength 70.0 MPa2 mm/min; ISO 178
Flexural Modulus 2400 MPa2 mm/min; ISO 178
Izod Impact, Notched (ISO) 11.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
 15.0 kJ/m²
@Temperature -20.0 °C
ISO 180-1A
 25.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 100 °CISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 96.0 °CISO 75-1,-2
Vicat Softening Point 102 °C
@Load 5.10 kg
120°C/hour; ISO 306
Flammability, UL94 HB
@Thickness 1.60 mm
 
Optical PropertiesOriginal ValueComments
Gloss 90 %Angle 60°; ISO 2813

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lotte Advanced Materials Starex® SV-0167 ABS, Unreinforced Extrusion Grade
Ineos ABS Lustran® LK197 ABS, Extrusion Grade
IRPC Polimaxx Porene SR101 Acrylonitrile Butadiene Styrene
Ineos ABS Lustran® H950
Ineos ABS Lustran® E401

PINEA946 / 107217

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.