MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Zytel® ST7301 BK356 PA6-HI
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Impact Grade

Material Notes: Super Toughened Polyamide 6

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.06 g/ccDAM; ISO 1183
Moisture Absorption 2.70 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.013 cm/cmDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.013 cm/cmDAM; ISO 294-4, 2577
Melt Flow 6.5 g/10 min
@Load 2.16 kg,
Temperature 250 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 30.0 MPa50% RH; ISO 527-1/-2
 48.0 MPaDAM; ISO 527-1/-2
Elongation at Break 45 %Nominal; DAM; ISO 527-1/-2
 >= 50 %Nominal; 50% RH; ISO 527-1/-2
Elongation at Yield 4.0 %DAM; ISO 527-1/-2
 33 %50% RH; ISO 527-1/-2
Tensile Modulus 550 MPa50% RH; ISO 527-1/-2
 1800 MPaDAM; ISO 527-1/-2
Flexural Modulus 550 MPa50% RH; ISO 178
 1800 MPaDAM; ISO 178
Poissons Ratio 0.41DAM
 0.4750% RH
Izod Impact, Notched (ISO) 12.0 kJ/m²
@Temperature -40.0 °C
50% RH; ISO 180/1A
 13.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 180/1A
 15.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 16.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 57.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 95.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact, Notched 14.0 kJ/m²
@Temperature -40.0 °C
50% RH; ISO 179/1eA
 16.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eA
 17.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 18.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 77.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 120 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Melting Point 221 °C10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 88.0 °CDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 45.0 °CDAM; ISO 75-1/-2
Glass Transition Temp, Tg 15.0 °C10°C/min; 50% RH; ISO 11357-1/-2
 60.0 °C10°C/min; DAM; ISO 11357-1/-2
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
 
Processing PropertiesOriginal ValueComments
Melt Temperature 240 °COptimum, Extrusion
 235 - 250 °CRange, Extrusion
 260 - 280 °CRange, Injection
 270 °COptimum, Injection
Mold Temperature 70.0 °COptimum, Injection
 50.0 - 90.0 °CInjection
Ejection Temperature 140 °CInjection
Drying Temperature 80.0 °CInjection
 80.0 °CExtrusion
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
 3.00 - 4.00 hourExtrusion, Dehumidified Dryer
Moisture Content <= 0.060 %Extrusion
 <= 0.20 %Injection
Hold Pressure 50.0 - 100 MPaRange, Injection
 
Descriptive Properties
Drying RecommendedyesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
ISO designationISO 16396-PA6-I,,M1CG1HR,S14-020
Max. screw tangential speed (m/s)0.3Injection
Part Marking Code>PA6-HI<ISO 11469
PolymerPA6-I
Processing Hold Pressure Time (s/mm)4Injection
Resin IdentificationPA6-HIISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Zytel® BM7300THS BK317 PA6-HI
Celanese Zytel® ST7301 NC010 PA6-HI
Ascend Performance Materials Vydyne® R515 Nylon 66, 15% Glass Filled
DuPont Mobility and Materials Zytel® 7301 NC010 PA6
Celanese Zytel® 103FHSA NC010 PA66

PDSX5505 / 198145

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.