MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 7178-T76; 7178-T7651
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 7000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A97178; Aluminium 7178-T76; Aluminium 7178-T7651; AA7178-T76; AA7178-T7651; Al7178-T76
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.83 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 152500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 193Converted from Brinell Hardness Value
Hardness, Rockwell A 53.9Converted from Brinell Hardness Value
Hardness, Rockwell B 88Converted from Brinell Hardness Value
Hardness, Vickers 177Converted from Brinell Hardness Value
Tensile Strength, Ultimate 83.0 ksiAA; Typical
 45.0 MPa
@Temperature 371 °C
 59.0 MPa
@Temperature 316 °C
 76.0 MPa
@Temperature 260 °C
 105 MPa
@Temperature 204 °C
 215 MPa
@Temperature 149 °C
 475 MPa
@Temperature 100 °C
 570 MPa
@Temperature 24.0 °C
 605 MPa
@Temperature -28.0 °C
 625 MPa
@Temperature -80.0 °C
 730 MPa
@Temperature -196 °C
Tensile Strength, Yield 73.0 ksiAA; Typical
 38.0 MPa
@Strain 0.2 %,
Temperature 271 °C
 48.0 MPa
@Strain 0.2 %,
Temperature 316 °C
 62.0 MPa
@Strain 0.2 %,
Temperature 260 °C
 83.0 MPa
@Strain 0.2 %,
Temperature 204 °C
 185 MPa
@Strain 0.2 %,
Temperature 149 °C
 440 MPa
@Strain 0.2 %,
Temperature 100 °C
 505 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 525 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 540 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 615 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 10 %
@Temperature -196 °C
 10 %
@Temperature -80.0 °C
 10 %
@Temperature -28.0 °C
 11 %
@Temperature 24.0 °C
 17 %
@Temperature 100 °C
 40 %
@Temperature 149 °C
 70 %
@Temperature 204 °C
 76 %
@Temperature 260 °C
 80 %
@Temperature 316 °C
 80 %
@Temperature 371 °C
 11 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 73.0 GPa
 10300 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Compressive Yield Strength 460 MPa0.1% Permanent Set
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 160 MPa
@# of Cycles 5.00e+8
Shear Modulus 27.0 GPaEstimated from similar Al alloys.
Shear Strength 340 MPaCalculated value.
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000500 ohm-cmEstimated from other heat treatments.
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.0 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 21.7 µm/m-°C
@Temperature -50.0 - 20.0 °C
 23.5 µm/m-°C
@Temperature 20.0 - 100 °C
 24.4 µm/m-°C
@Temperature 20.0 - 200 °C
 25.4 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.856 J/g-°C
Thermal Conductivity 140 W/m-KEstimated from other heat treatments.
Melting Point 890 - 1165 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Homogenization may raise eutectic melting temperature 20-40°F but usually does not eliminate it.
Solidus 890 °FAA; Typical
Liquidus 1165 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 875 °F
Aging Temperature 250 °Ffor 24 hr
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 85.3 - 89.5 %As remainder
Chromium, Cr 0.18 - 0.28 %
Copper, Cu 1.6 - 2.4 %
Iron, Fe <= 0.50 %
Magnesium, Mg 2.4 - 3.1 %
Manganese, Mn <= 0.30 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.40 %
Titanium, Ti <= 0.20 %
Zinc, Zn 6.3 - 7.3 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 7178-T6; 7178-T651
Aluminum 7075-T6; 7075-T651
Aluminum 7178-T6; 7178-T651 (Included Creep/Rupture Data)
Aluminum 7475-T7651
Aluminum 7175-T736; 7175-T7365x

MA7178T76 / 9621

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.