MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Titanium Ti-8Mn, Annealed
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Beta Titanium Alloy

Material Notes: Annealed 705ºC. Alpha-Beta Alloy. Not weldable.

Applications: Aircraft, structural parts

Key Words: UNS R56080
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 4.73 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 318Estimated from Rockwell C.
Hardness, Knoop 346Estimated from Rockwell C.
Hardness, Rockwell C 34
Hardness, Vickers 333Estimated from Rockwell C.
Tensile Strength, Ultimate 900 MPa
Tensile Strength, Yield 810 MPa
Elongation at Break 14 %
Reduction of Area 32 %
Creep Strength 200 MPa
@Temperature 425 °C,
Time >=21600 sec
strain 0.5%
 200 MPa
@Temperature 425 °C,
Time >=2880 sec
strain 0.1%
 400 MPa
@Temperature 370 °C,
Time >=216000 sec
strain 0.5%
 400 MPa
@Temperature 370 °C,
Time >=21600 sec
strain 0.1%
Rupture Strength >= 250 MPa
@Temperature 425 °C,
Time 360000 sec
 600 MPa
@Temperature 370 °C,
Time 360000 sec
 >= 800 MPa
@Temperature 315 °C,
Time 360000 sec
Modulus of Elasticity 115 GPaTypical value for annealed alpha/beta titanium alloy.
Modulus of Rigidity 48.3 GPa
Compressive Yield Strength 875 MPa
Poissons Ratio 0.33Typical for alpha-beta titanium alloy.
Fatigue Strength 210 MPa
@# of Cycles 1.00e+7
Rotating Beam. Kt (stress concentration factor) = 3.0
 400 MPa
@# of Cycles 10000
Rotating Beam. Kt (stress concentration factor) = 3.0
 585 MPa
@# of Cycles 1.00e+7
Unnotched Sheet
 800 MPa
@# of Cycles 2000
unnotched
Shear Modulus 43.2 GPaCalculated from typical values.
Bend Radius, Minimum 3.0 t
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000920 ohm-cm
Magnetic Permeability 1.00005at 1.6 kA/m
 
Thermal PropertiesOriginal ValueComments
CTE, linear 8.60 µm/m-°C
@Temperature 20.0 - 100 °C
 9.70 µm/m-°C
@Temperature 20.0 - 315 °C
average
 11.7 µm/m-°C
@Temperature 20.0 - 650 °C
average
Specific Heat Capacity 0.495 J/g-°C
Thermal Conductivity 10.9 W/m-K
@Temperature 20.0 °C
 12.8 W/m-K
@Temperature 205 °C
 15.2 W/m-K
@Temperature 425 °C
 17.8 W/m-K
@Temperature 650 °C
Melting Point 1565 °C
Solidus 1300 °C
Liquidus 1635 °C
Beta Transus 785 - 815 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.20 %
Hydrogen, H <= 0.015 %
Manganese, Mn 8.0 %
Nitrogen, N <= 0.070 %
Oxygen, O <= 0.20 %
Titanium, Ti 92 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2024-T3
Medical Grade Stainless Steel 316LVM
Sandvik Bioline 316LVM Tube and pipe, seamless
Overview of materials for Alpha/Beta Titanium Alloy
Ti6Al7Nb ASTM F1295

MTP081 / 14226

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.