MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ATI Allegheny Ludlum 310S Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Stainless Steel; T 300 Series Stainless Steel

Material Notes: Comparable corrosion resistance, superior resistance to oxidation, and the retention of a larger fraction of room temperature strength than common austenitic alloys. Good creep deformation resistance.

Applications:Heat treatment industry-conveyor belts, rollers, burner parts, refractory supports, retorts linings, oven linings, fans, tube hangers, baskets, and trays. Chemical process industry- containers for hot concentrated acids, ammonia, and sulfur dioxide. Food processing industry- used in contact with hot acetic and citric acid.

Typical mechanical property data reported.

Key Words: UNS S31008
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.03 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 624 MPaASTM E8
 44.0 MPa
@Temperature 1093 °C
ASTM E8
 81.0 MPa
@Temperature 982 °C
ASTM E8
 155 MPa
@Temperature 871 °C
ASTM E8
 393 MPa
@Temperature 649 °C
ASTM E8
 484 MPa
@Temperature 538 °C
ASTM E8
 508 MPa
@Temperature 427 °C
ASTM E8
 533 MPa
@Temperature 204 °C
ASTM E8
Tensile Strength, Yield 27.0 MPa
@Temperature 1093 °C
ASTM E8
 56.0 MPa
@Temperature 982 °C
ASTM E8
 111 MPa
@Temperature 871 °C
ASTM E8
 178 MPa
@Temperature 649 °C
ASTM E8
 203 MPa
@Temperature 538 °C
ASTM E8
 209 MPa
@Temperature 427 °C
ASTM E8
 254 MPa
@Temperature 204 °C
ASTM E8
 314 MPa
@Strain 0.2 %
ASTM E8
Elongation at Break 42.6 %ASTM E8
 32 %
@Temperature 649 °C
ASTM E8
 33.5 %
@Temperature 427 °C
ASTM E8
 35.8 %
@Temperature 204 °C
ASTM E8
 37 %
@Temperature 538 °C
ASTM E8
 56.5 %
@Temperature 871 °C
ASTM E8
 93.3 %
@Temperature 982 °C
ASTM E8
 121 %
@Temperature 1093 °C
ASTM E8
Creep Strength 20.0 MPa
@Temperature 788 °C,
Time 3.60e+7 sec
1% creep
 138 MPa
@Temperature 593 °C,
Time 3.60e+7 sec
1% creep
Rupture Strength 20.0 MPa
@Temperature 899 °C,
Time 3.60e+7 sec
 138 MPa
@Temperature 593 °C,
Time 3.60e+7 sec
Modulus of Elasticity 200 GPa
Poissons Ratio 0.30calculated
Shear Modulus 77.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000780 ohm-cm
@Temperature 20.0 °C
Magnetic Permeability 1.02at 200H
 
Thermal PropertiesOriginal ValueComments
CTE, linear 15.9 µm/m-°C
@Temperature 20.0 - 100 °C
 17.1 µm/m-°C
@Temperature 20.0 - 500 °C
 18.9 µm/m-°C
@Temperature 20.0 - 1000 °C
Specific Heat Capacity 0.502 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 13.8 W/m-K
@Temperature 20.0 - 100 °C
 18.7 W/m-K
@Temperature 20.0 - 500 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.0800 %
Chromium, Cr 24 - 26 %
Iron, Fe 48 - 57 %As Remainder
Manganese, Mn <= 2.00 %
Nickel, Ni 19 - 22 %
Phosphorus, P <= 0.0450 %
Silicon, Si <= 1.50 %
Sulfur, S <= 0.0300 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type 310S Stainless Steel
ATI Allegheny Ludlum 310H Austenitic Stainless Steel
310 Stainless Steel, annealed sheet
ATI Allegheny Ludlum 310 Austenitic Stainless Steel
Industeel SIRIUS 310 25% Cr - 0.6% Si Heat Resistant Stainless Steel

NL1005 / 17773

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.