MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aluminum 2219-T37
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92219; ISO AlCu6Mn; Aluminium 2219-T37; AA2219-T37; Al2219-T37
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.84 g/cc0.103 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 117117500 kg load with 10 mm ball
Hardness, Knoop 146146Converted from Brinell Hardness Value
Hardness, Rockwell A 45.845.8Converted from Brinell Hardness Value
Hardness, Rockwell B 7373Converted from Brinell Hardness Value
Hardness, Vickers 133133Converted from Brinell Hardness Value
Tensile Strength, Ultimate 393 MPa57000 psiAA; Typical
 >= 295 MPa
@Thickness 101.6 - 127 mm
>= 42800 psi
@Thickness 4.001 - 5.00 in
Sheet and plate
 >= 310 MPa
@Thickness 76.23 - 102 mm
>= 45000 psi
@Thickness 3.001 - 4.00 in
Sheet and plate
 >= 325 MPa
@Thickness 63.53 - 76.2 mm
>= 47100 psi
@Thickness 2.501 - 3.00 in
Sheet and plate
 >= 340 MPa
@Thickness 0.508 - 0.991 mm
>= 49300 psi
@Thickness 0.0200 - 0.0390 in
Sheet and plate
 >= 340 MPa
@Thickness 1.02 - 63.5 mm
>= 49300 psi
@Thickness 0.0400 - 2.50 in
Sheet and plate
Tensile Strength, Yield 317 MPa46000 psiAA; Typical
 >= 235 MPa
@Thickness 101.6 - 127 mm
>= 34100 psi
@Thickness 4.001 - 5.00 in
Sheet and plate
 >= 240 MPa
@Thickness 76.23 - 102 mm
>= 34800 psi
@Thickness 3.001 - 4.00 in
Sheet and plate
 >= 250 MPa
@Thickness 63.53 - 76.2 mm
>= 36300 psi
@Thickness 2.501 - 3.00 in
Sheet and plate
 >= 255 MPa
@Thickness 1.02 - 63.5 mm
>= 37000 psi
@Thickness 0.0400 - 2.50 in
Sheet and plate
 >= 260 MPa
@Thickness 0.508 - 0.991 mm
>= 37700 psi
@Thickness 0.0200 - 0.0390 in
Sheet and plate
Elongation at Break  4.0 %
@Thickness 101.6 - 127 mm
4.0 %
@Thickness 4.001 - 5.00 in
Sheet and plate
 5.0 %
@Thickness 76.23 - 102 mm
5.0 %
@Thickness 3.001 - 4.00 in
Sheet and plate
 6.0 %
@Thickness 0.508 - 0.991 mm
6.0 %
@Thickness 0.0200 - 0.0390 in
Sheet and plate
 6.0 %
@Thickness 1.02 - 63.5 mm
6.0 %
@Thickness 0.0400 - 2.50 in
Sheet and plate
 6.0 %
@Thickness 63.53 - 76.2 mm
6.0 %
@Thickness 2.501 - 3.00 in
Sheet and plate
 11 %
@Thickness 1.59 mm
11 %
@Thickness 0.0625 in
AA; Typical
Modulus of Elasticity 73.1 GPa10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Shear Modulus 27.0 GPa3920 ksiEstimated from similar Al alloys.
Shear Strength 255 MPa37000 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000615 ohm-cm
@Temperature 20.0 °C
0.00000615 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
11.6 µin/in-°F
@Temperature -58.0 - 68.0 °F
 22.3 µm/m-°C
@Temperature 20.0 - 100 °C
12.4 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
12.5 µin/in-°F
@Temperature 68.0 - 212 °F
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
13.0 µin/in-°F
@Temperature 68.0 - 392 °F
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
13.4 µin/in-°F
@Temperature 68.0 - 572 °F
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
13.6 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.864 J/g-°C0.207 BTU/lb-°F
Thermal Conductivity 112 W/m-K780 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 543 - 643 °C1010 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 543 °C1010 °FAA; Typical
Liquidus 643 °C1190 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °F
Solution Temperature 535 °C995 °F
Aging Temperature 163 - 191 °C325 - 375 °Ffrom 18 to 36 hr at temperature
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 91.5 - 93.8 %91.5 - 93.8 %As remainder
Copper, Cu 5.8 - 6.8 %5.8 - 6.8 %
Iron, Fe <= 0.30 %<= 0.30 %
Magnesium, Mg <= 0.02 %<= 0.02 %
Manganese, Mn 0.20 - 0.40 %0.20 - 0.40 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.20 %<= 0.20 %
Titanium, Ti 0.02 - 0.10 %0.02 - 0.10 %
Vanadium, V 0.05 - 0.15 %0.05 - 0.15 %
Zinc, Zn <= 0.10 %<= 0.10 %
Zirconium, Zr 0.10 - 0.25 %0.10 - 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 2219-T87
Aluminum 2219-T31
Aluminum 2219-T351
Aluminum 2219-O
Aluminum 2219-T6

MA2219T37 / 8929

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.