MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Alloy Cast Iron
Categories: Metal; Ferrous Metal; Cast Iron; Alloy Cast Iron

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Alloy Cast Iron". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 5.54 - 7.81 g/ccAverage value: 7.17 g/cc Grade Count:84
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 110 - 807Average value: 262 Grade Count:77
Hardness, Knoop 162 - 906Average value: 252 Grade Count:34
Hardness, Rockwell C 11.6 - 65.0Average value: 31.8 Grade Count:11
Hardness, Vickers 151 - 871Average value: 238 Grade Count:34
Tensile Strength, Ultimate 90.0 - 1650 MPaAverage value: 632 MPa Grade Count:86
Tensile Strength, Yield 172 - 1450 MPaAverage value: 520 MPa Grade Count:72
Elongation at Break 0.200 - 40.0 %Average value: 9.06 % Grade Count:66
Reduction of Area 2.00 - 10.0 %Average value: 5.38 % Grade Count:13
Modulus of Elasticity 63.0 - 240 GPaAverage value: 156 GPa Grade Count:38
Compressive Yield Strength 331 - 2520 MPaAverage value: 1050 MPa Grade Count:23
Poissons Ratio 0.250 - 0.370Average value: 0.283 Grade Count:23
Fatigue Strength 68.9 - 510 MPaAverage value: 334 MPa Grade Count:18
Fracture Toughness 44.0 - 110 MPa-m½Average value: 81.4 MPa-m½ Grade Count:7
Machinability 0.000 - 125 %Average value: 41.7 % Grade Count:3
Shear Modulus 60.2 - 67.6 GPaAverage value: 64.5 GPa Grade Count:23
Shear Strength 200 - 1480 MPaAverage value: 712 MPa Grade Count:15
Charpy Impact 0.100 - 40.0 JAverage value: 15.3 J Grade Count:13
Charpy Impact, Unnotched 2.70 - 200 JAverage value: 78.0 J Grade Count:22
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000500 - 110 ohm-cmAverage value: 6.11 ohm-cm Grade Count:18
Magnetic Permeability 100 - 750Average value: 410 Grade Count:5
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.75 - 19.3 µm/m-°CAverage value: 12.7 µm/m-°C Grade Count:29
Specific Heat Capacity 0.506 J/g-°CAverage value: 0.506 J/g-°C Grade Count:3
Thermal Conductivity 11.3 - 53.3 W/m-KAverage value: 26.6 W/m-K Grade Count:23
Melting Point 1120 - 1310 °CAverage value: 1150 °C Grade Count:8
Maximum Service Temperature, Air 649 °CAverage value: 649 °C Grade Count:6
Minimum Service Temperature, Air -59.4 - -30.0 °CAverage value: -34.9 °C Grade Count:6
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.0500 - 25.0 %Average value: 3.26 % Grade Count:7
Antimony, Sb 0.00200 - 0.200 %Average value: 0.0174 % Grade Count:7
Arsenic, As 0.0200 %Average value: 0.0200 % Grade Count:6
Bismuth, Bi 0.00200 %Average value: 0.00200 % Grade Count:6
Boron, B 0.000600 %Average value: 0.000600 % Grade Count:6
Cadmium, Cd 0.00500 %Average value: 0.00500 % Grade Count:6
Carbon, C 0.400 - 4.10 %Average value: 3.25 % Grade Count:77
Cerium, Ce 0.00500 - 0.200 %Average value: 0.102 % Grade Count:24
Chromium, Cr 0.0300 - 35.0 %Average value: 2.48 % Grade Count:60
Copper, Cu 0.0200 - 10.0 %Average value: 1.23 % Grade Count:50
Iron, Fe 49.0 - 96.2 %Average value: 84.7 % Grade Count:85
Lead, Pb 0.00200 %Average value: 0.00200 % Grade Count:6
Magnesium, Mg 0.0200 - 0.0600 %Average value: 0.0425 % Grade Count:30
Manganese, Mn 0.100 - 4.50 %Average value: 0.679 % Grade Count:74
Molybdenum, Mo 0.000 - 16.0 %Average value: 0.759 % Grade Count:54
Nickel, Ni 0.0500 - 43.0 %Average value: 8.62 % Grade Count:59
Oxygen, O 0.00500 %Average value: 0.00500 % Grade Count:6
Phosphorus, P 0.0150 - 0.300 %Average value: 0.0782 % Grade Count:67
Selenium, Se 0.0300 %Average value: 0.0300 % Grade Count:6
Silicon, Si 0.500 - 17.0 %Average value: 2.77 % Grade Count:85
Sulfur, S 0.00200 - 0.150 %Average value: 0.0463 % Grade Count:57
Tellurium, Te 0.0200 %Average value: 0.0200 % Grade Count:6
Tin, Sn 0.0100 - 0.300 %Average value: 0.0538 % Grade Count:12
Titanium, Ti 0.0400 %Average value: 0.0400 % Grade Count:6
Vanadium, V 0.100 - 2.00 %Average value: 0.478 % Grade Count:9

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Cast Iron
Overview of materials for Stainless Steel
Overview of materials for Aluminum Alloy
Overview of materials for Cast Stainless Steel
Overview of materials for T 400 Series Stainless Steel

M01013 / 81711

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.