MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 6101-T6
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A96101; ISO E-AlMgSi; Aluminium 6101-T6; AA6101-T6; Al6101-T6
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.70 g/cc0.0975 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 7171AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 9494Converted from Brinell Hardness Value
Hardness, Vickers 8181Converted from Brinell Hardness Value
Tensile Strength, Ultimate 221 MPa32000 psiAA; Typical
 17.0 MPa
@Temperature 371 °C
2470 psi
@Temperature 700 °F
 24.0 MPa
@Temperature 316 °C
3480 psi
@Temperature 601 °F
 33.0 MPa
@Temperature 260 °C
4790 psi
@Temperature 500 °F
 69.0 MPa
@Temperature 204 °C
10000 psi
@Temperature 399 °F
 145 MPa
@Temperature 149 °C
21000 psi
@Temperature 300 °F
 193 MPa
@Temperature 100 °C
28000 psi
@Temperature 212 °F
 221 MPa
@Temperature 24.0 °C
32100 psi
@Temperature 75.2 °F
 234 MPa
@Temperature -28.0 °C
33900 psi
@Temperature -18.4 °F
 248 MPa
@Temperature -80.0 °C
36000 psi
@Temperature -112 °F
 296 MPa
@Temperature -196 °C
42900 psi
@Temperature -321 °F
Tensile Strength, Yield 193 MPa28000 psiAA; Typical
 12.0 MPa
@Strain 0.2 %,
Temperature 371 °C
1740 psi
@Strain 0.2 %,
Temperature 700 °F
 16.0 MPa
@Strain 0.2 %,
Temperature 316 °C
2320 psi
@Strain 0.2 %,
Temperature 601 °F
 23.0 MPa
@Strain 0.2 %,
Temperature 260 °C
3340 psi
@Strain 0.2 %,
Temperature 500 °F
 48.0 MPa
@Strain 0.2 %,
Temperature 204 °C
6960 psi
@Strain 0.2 %,
Temperature 399 °F
 131 MPa
@Strain 0.2 %,
Temperature 149 °C
19000 psi
@Strain 0.2 %,
Temperature 300 °F
 172 MPa
@Strain 0.2 %,
Temperature 100 °C
24900 psi
@Strain 0.2 %,
Temperature 212 °F
 193 MPa
@Strain 0.2 %,
Temperature 24.0 °C
28000 psi
@Strain 0.2 %,
Temperature 75.2 °F
 200 MPa
@Strain 0.2 %,
Temperature -28.0 °C
29000 psi
@Strain 0.2 %,
Temperature -18.4 °F
 207 MPa
@Strain 0.2 %,
Temperature -80.0 °C
30000 psi
@Strain 0.2 %,
Temperature -112 °F
 228 MPa
@Strain 0.2 %,
Temperature -196 °C
33100 psi
@Strain 0.2 %,
Temperature -321 °F
Elongation at Break  19 %
@Temperature -28.0 °C
19 %
@Temperature -18.4 °F
 19 %
@Temperature 24.0 °C
19 %
@Temperature 75.2 °F
 20 %
@Temperature -80.0 °C
20 %
@Temperature -112 °F
 20 %
@Temperature 100 °C
20 %
@Temperature 212 °F
 20 %
@Temperature 149 °C
20 %
@Temperature 300 °F
 24 %
@Temperature -196 °C
24 %
@Temperature -321 °F
 40 %
@Temperature 204 °C
40 %
@Temperature 399 °F
 80 %
@Temperature 260 °C
80 %
@Temperature 500 °F
 100 %
@Temperature 316 °C
100 %
@Temperature 601 °F
 105 %
@Temperature 371 °C
105 %
@Temperature 700 °F
 15 %
@Thickness 1.59 mm
15 %
@Thickness 0.0625 in
AA; Typical
Modulus of Elasticity 68.9 GPa10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Machinability 50 %50 %0-100 Scale of Aluminum Alloys
Shear Modulus 26.0 GPa3770 ksiEstimated from similar Al alloys.
Shear Strength 138 MPa20000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000299 ohm-cm
@Temperature 20.0 °C
0.00000299 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  21.7 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.1 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.4 µm/m-°C
@Temperature 20.0 - 100 °C
13.0 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 23.5 µm/m-°C
@Temperature 20.0 - 100 °C
13.1 µin/in-°F
@Temperature 68.0 - 212 °F
 24.4 µm/m-°C
@Temperature 20.0 - 200 °C
13.6 µin/in-°F
@Temperature 68.0 - 392 °F
 25.4 µm/m-°C
@Temperature 20.0 - 300 °C
14.1 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.895 J/g-°C0.214 BTU/lb-°F
Thermal Conductivity 218 W/m-K1510 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 621 - 654 °C1150 - 1210 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 621 °C1150 °FAA; Typical
Liquidus 654 °C1210 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Solution Temperature 510 °C950 °Fhold at temperature for 1 hr
Aging Temperature 177 °C350 °Fhold at temperature for 6 to 8 hr
Hot-Working Temperature 260 - 510 °C500 - 950 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 97.6 %<= 97.6 %As remainder
Boron, B <= 0.06 %<= 0.06 %
Chromium, Cr <= 0.03 %<= 0.03 %
Copper, Cu <= 0.10 %<= 0.10 %
Iron, Fe <= 0.50 %<= 0.50 %
Magnesium, Mg 0.35 - 0.80 %0.35 - 0.80 %
Manganese, Mn <= 0.03 %<= 0.03 %
Other, each <= 0.03 %<= 0.03 %
Other, total <= 0.10 %<= 0.10 %
Silicon, Si 0.30 - 0.70 %0.30 - 0.70 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 6063-T6
Aluminum 6101-H111
Aluminum 6101-T61
Aluminum 6351-T6; 6351-T651

MA6101T6 / 9442

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.