MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

HOS-Technik Homide 250 Bismaleimide Resin
Categories: Polymer; Thermoset; Bismaleimide (BMI)

Material Notes: Homide 250 is a prepolymer bismaleimide resin system with a low softening range of 90-125°C supplied in powder form. The resin can be cured thermally to create a cross-linked thermoset with excellent thermal and mechanical resistance. Homide 250 can be processed in powder form or dissolved in an organic solvent, such as dimethylformamide or N-methylpyrrolidone, up to a concentration of 45% for the production of composite materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.95 g/cc0.0704 lb/in³EN 60893
Water Absorption 0.10 %0.10 %EN 60893
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 300 MPa
@Thickness >=1.60 mm
43500 psi
@Thickness >=0.0630 in
EN 60893
Modulus of Elasticity 25.0 GPa
@Thickness >=1.60 mm
3630 ksi
@Thickness >=0.0630 in
EN 60893
Flexural Strength  360 MPa
@Thickness >=1.60 mm,
Temperature 200 °C
52200 psi
@Thickness >=0.0630 in,
Temperature 392 °F
Perpendicular to laminations; EN 60893
 425 MPa
@Thickness >=1.60 mm,
Temperature 150 °C
61600 psi
@Thickness >=0.0630 in,
Temperature 302 °F
Perpendicular to laminations; EN 60893
 475 MPa
@Thickness >=1.60 mm,
Temperature 100 °C
68900 psi
@Thickness >=0.0630 in,
Temperature 212 °F
Perpendicular to laminations; EN 60893
 500 MPa
@Thickness >=1.60 mm,
Temperature 20.0 °C
72500 psi
@Thickness >=0.0630 in,
Temperature 68.0 °F
Perpendicular to laminations; EN 60893
 500 MPa
@Thickness >=1.60 mm,
Temperature 50.0 °C
72500 psi
@Thickness >=0.0630 in,
Temperature 122 °F
Perpendicular to laminations; EN 60893
Compressive Strength  440 MPa
@Thickness >=5.00 mm,
Temperature 200 °C
63800 psi
@Thickness >=0.197 in,
Temperature 392 °F
Perpendicular to laminations; EN 60893
 480 MPa
@Thickness >=5.00 mm,
Temperature 150 °C
69600 psi
@Thickness >=0.197 in,
Temperature 302 °F
Perpendicular to laminations; EN 60893
 550 MPa
@Thickness >=5.00 mm,
Temperature 100 °C
79800 psi
@Thickness >=0.197 in,
Temperature 212 °F
Perpendicular to laminations; EN 60893
 620 MPa
@Thickness >=5.00 mm,
Temperature 50.0 °C
89900 psi
@Thickness >=0.197 in,
Temperature 122 °F
Perpendicular to laminations; EN 60893
 650 MPa
@Thickness >=5.00 mm,
Temperature 20.0 °C
94300 psi
@Thickness >=0.197 in,
Temperature 68.0 °F
Perpendicular to laminations; EN 60893
Shear Strength 70.0 MPa
@Thickness >=5.00 mm
10200 psi
@Thickness >=0.197 in
Parallel to laminations; EN 60893
Izod Impact Resistance 5.50 J/cm²
@Thickness >=127 mm
26.2 ft-lb/in²
@Thickness >=5.00 in
Parallel to laminations; EN 60893
 
Electrical PropertiesMetricEnglishComments
Insulation Resistance 1.00e+6 ohm1.00e+6 ohmAfter immersion in water; EN 60893
Dielectric Constant 4.0
@Thickness >=3.00 mm,
Frequency 50 Hz
4.0
@Thickness >=0.118 in,
Frequency 50 Hz
EN 60893
Dielectric Strength 20.0 kV/mm
@Thickness >=3.00 mm,
Temperature 90.0 °C
508 kV/in
@Thickness >=0.118 in,
Temperature 194 °F
Tested in oil. Perpendicular to laminations.; EN 60893
Dissipation Factor 0.010
@Thickness >=3.00 mm,
Frequency 50 Hz
0.010
@Thickness >=0.118 in,
Frequency 50 Hz
EN 60893
 
Thermal PropertiesMetricEnglishComments
Flammability, UL94 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
EN 60893

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Hexcel® HexPly® F650 Bismaleimide Resin
Solvay HTM® 556 BMI
Solvay HTM® 552 Bismaleimide Resin
Hexcel® HexPly® F652 Bismaleimide Resin
Evonik Compimide® 353A Bismaleimide

PHOS990 / 123934

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.