MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2219-T62
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92219; ISO AlCu6Mn; Aluminium 2219-T62; AA2219-T62; Al2219-T62
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.84 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 115500 kg load with 10 mm ball
Hardness, Knoop 145Converted from Brinell Hardness Value
Hardness, Rockwell A 45.5Converted from Brinell Hardness Value
Hardness, Rockwell B 72Converted from Brinell Hardness Value
Hardness, Vickers 130Converted from Brinell Hardness Value
Tensile Strength, Ultimate 60.0 ksiAA; Typical
 >= 370 MPaSheet and plate
 >= 370 MPaWire, rod, bar, and shapes (extruded)
 >= 370 MPaExtruded tube
 30.0 MPa
@Temperature 371 °C
 69.0 MPa
@Temperature 316 °C
 186 MPa
@Temperature 260 °C
 234 MPa
@Temperature 204 °C
 310 MPa
@Temperature 149 °C
 372 MPa
@Temperature 100 °C
 400 MPa
@Temperature 24.0 °C
 414 MPa
@Temperature -28.0 °C
 434 MPa
@Temperature -80.0 °C
 503 MPa
@Temperature -196 °C
Tensile Strength, Yield 42.0 ksiAA; Typical
 >= 250 MPaSheet and plate
 >= 250 MPaWire, rod, bar, and shapes (extruded)
 >= 250 MPaExtruded tube
 26.0 MPa
@Strain 0.2 %,
Temperature 371 °C
 55.0 MPa
@Strain 0.2 %,
Temperature 316 °C
 133 MPa
@Strain 0.2 %,
Temperature 260 °C
 172 MPa
@Strain 0.2 %,
Temperature 204 °C
 227 MPa
@Strain 0.2 %,
Temperature 149 °C
 255 MPa
@Strain 0.2 %,
Temperature 100 °C
 276 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 290 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 303 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 338 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 6.0 %Wire, rod, bar, and shapes (extruded)
 6.0 %Extruded tube
 6.0 - 8.0 %Sheet and plate
 12 %
@Temperature -28.0 °C
 12 %
@Temperature 24.0 °C
 13 %
@Temperature -80.0 °C
 14 %
@Temperature 100 °C
 16 %
@Temperature -196 °C
 17 %
@Temperature 149 °C
 20 %
@Temperature 204 °C
 21 %
@Temperature 260 °C
 40 %
@Temperature 316 °C
 75 %
@Temperature 371 °C
 10 %
@Thickness 1.59 mm
AA; Typical
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 15000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPaEstimated from similar Al alloys.
Shear Strength 255 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000570 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.864 J/g-°C
Thermal Conductivity 120 W/m-K
Melting Point 1010 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 1010 °FAA; Typical
Liquidus 1190 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 995 °F
Aging Temperature 325 - 375 °Ffrom 18 to 36 hr at temperature
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 91.5 - 93.8 %As remainder
Copper, Cu 5.8 - 6.8 %
Iron, Fe <= 0.30 %
Magnesium, Mg <= 0.02 %
Manganese, Mn 0.20 - 0.40 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.20 %
Titanium, Ti 0.02 - 0.10 %
Vanadium, V 0.05 - 0.15 %
Zinc, Zn <= 0.10 %
Zirconium, Zr 0.10 - 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2219-T6
Aluminum 2219-T81
Aluminum 2219-T851
Aluminum 2219-T851 (Extended High Temperature Data)
Aluminum 2219-O

MA2219T62 / 8932

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.