System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Samyang Triel® 5700 Thermoplastics Polyetherester Elastomer, General Extrusion
Categories:
Polymer
;
Thermoplastic
;
Elastomer, TPE
;
Polyester, TP
;
Polyether Ester Elastomer
Material Notes:
Excellent mechanical characteristics, elasticity, thermal resistance and chemical resistance.
5700 is an extrusion grade.
Information provided by Samyang.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.25
g/cc
1.25
g/cc
ASTM D792
Water Absorption
0.50 %
0.50 %
ASTM D570
Linear Mold Shrinkage
0.017
-
0.020
cm/cm
0.017
-
0.020
in/in
ASTM D955
Melt Flow
6.0
g/10 min
@Load 2.16 kg,
Temperature 230 °C
6.0
g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
6.0
g/10 min
@Load 2.16 kg,
Temperature 240 °C
6.0
g/10 min
@Load 4.76 lb,
Temperature 464 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Hardness, Shore D
70
70
ASTM D2240
Tensile Strength, Ultimate
39.2
MPa
5690
psi
ASTM D638
Tensile Stress at Strain
23.5
MPa
@Strain 5.0 %
3410
psi
@Strain 5.0 %
ASTM D638
25.3
MPa
@Strain 50 %
3670
psi
@Strain 50 %
ASTM D638
27.9
MPa
@Strain 10 %
4050
psi
@Strain 10 %
ASTM D638
Flexural Yield Strength
24.5
MPa
3560
psi
ASTM D790
Flexural Modulus
0.608
GPa
88.2
ksi
ASTM D790
Izod Impact, Notched
0.686
-
0.883
J/cm
@Thickness 3.17 mm,
Temperature -40.0 °C
1.29
-
1.65
ft-lb/in
@Thickness 0.125 in,
Temperature -40.0 °F
ASTM D256
0.981
-
1.18
J/cm
@Thickness 3.17 mm,
Temperature 23.0 °C
1.84
-
2.20
ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
ASTM D256
Thermal Properties
Metric
English
Comments
Melting Point
215
°C
419
°F
ASTM D2117
Deflection Temperature at 0.46 MPa (66 psi)
118
°C
244
°F
ASTM D648
Vicat Softening Point
204
°C
399
°F
ASTM D1525
Descriptive Properties
Flexible Rate
> 400%
ASTM D638
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Samyang Triel® 5400 Thermoplastic Polyether Ester Elastomer
Samyang Triel® 5300 Thermoplastic Polyether Ester Elastomer
Samyang Triel® 5407EF Thermoplastic Polyether Ester Elastomer
Radici Heraform® R 1300 Acetal Copolymer
Radici Heraflex® P 40D 11 I HF 1530 Modified Polypropylene
PSANX949 / 133343
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.