MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Westlake EMAC® Plus SP1501 20% EMA Copolymer
Categories: Polymer; Thermoplastic; Ethylene Methyl Acrylate

Material Notes: Westlake EMAC� Plus SP1501 is a 20% EMA copolymer designed for extrusion coating, compounding, and blending where low viscosity, flexibility, and strength are important. SP1501 provides excellent elasticity and low temperature performance. This resin is capable of very high filler loadings. A higher peak melting temperature than comparable EMA grades makes it a more viable choice for building products that are subjected to 180�F testing. It has good adhesion to various substrates and is compatible with numerous resins. SP1501 is soft, flexible, and tough without plasticizers. Its applications include: extrusion coating, compounding, hot melt adhesives, compatibilizer, and concentrate base. This resin grade complies with 21 CFR 177.1340. EMAC� resins adhere to and are compatible with a wide range of materials including paper, polyolefins, oriented polyolefins, polyesters, ionomers, PVC, unplasticized PVC, and other polar polymers. They are made for use as a heat seal layer, adhesive layer, or modifier for cost/performance enhancement. They are soft, pliable, and tough at ambient and freezing temperatures and exhibit excellent ESCR. These polymers exhibit high solids fillability and compatibility with a wide range of polymers. This facilitates their uses as bases for all-purpose concentrates for addition to a wide spectrum of polymers. They process like LDPE.

Key Words: Excellent elasticity and low temperature performance.
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.941 g/ccASTM-D1505
Melt Flow 25 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM-D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 37ASTM-D2240
Tensile Strength at Break 800 psi500 mm/min (20 in./min); ASTM-D638 Type IV Specimen
Tensile Strength, Yield 560 psi500 mm/min (20 in./min); ASTM-D638 Type IV Specimen
Elongation at Break 480 %500 mm/min (20 in./min); ASTM-D638 Type IV Specimen
 
Thermal PropertiesOriginal ValueComments
Melting Point 100 °CDSC; ASTM-D3418
Vicat Softening Point 43.0 °CASTM-D1525
Brittleness Temperature <= -73.0 °CASTM-D746
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.
 
Descriptive Properties
Methyl Acrylate Content (%)20
processExtrusion

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow Engage® 8401 Polyolefin Elastomer
Westlake Epolene® E-43 Chemically Modified Polypropylene, Maleation Processed
Westlake EMAC® SP2404 18.5% EMA Copolymer
Westlake EMAC® SP2409 20% EMA Copolymer
Dow Elvaloy® AC 12024S Ethylene Methyl Acrylate

PWESF9007 / 106844

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.