MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2014-T6; 2014-T651 (Extended Form Data)
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Used in applications requiring high strength/hardness, including elevated temperature uses. Specific applications include heavy duty forgings, plate, and extrusions for aerospace fittings, wheels, tanks, and major structural components, heavy duty automotive frame and suspension componentry. 2014 exhibits poor corrosion resistance for an aluminum alloy.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
A Zr + Ti limit of 0.20 percent maximum may be used with this alloy designation for extruded and forged products only, but only when the supplier or producer and the purchaser have mutually so agreed. Agreement may be indicated, for example, by reference to a standard, by letter, by order note, or other means which allow the Zr + Ti limit.
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 2014-T651; UNS A92014; ISO AlCu4SiMg; BS H15 (UK); CSA CS41N (Canada); AA2014-T651, DIN AlCuSiMn; NF A-U4SG (France)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.80 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 135AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 170Converted from Brinell Hardness Value
Hardness, Rockwell A 50.5Converted from Rockwell B
Hardness, Rockwell B 82
Hardness, Vickers 155Converted from Brinell Hardness Value
Tensile Strength, Ultimate 70.0 ksiAA; Typical
 >= 415 MPaExtruded wire, rod, bar, and shapes; T62
 >= 415 MPaExtruded tube; T62
 >= 450 MPaRolled or cold finished wire (rod and bar); T6, T62, T651
 30.0 MPa
@Temperature 371 °C
 45.0 MPa
@Temperature 316 °C
 66.0 MPa
@Temperature 260 °C
 110 MPa
@Temperature 204 °C
 276 MPa
@Temperature 149 °C
 439 MPa
@Temperature 100 °C
 483 MPa
@Temperature 24.0 °C
 496 MPa
@Temperature -28.0 °C
 510 MPa
@Temperature -80.0 °C
 579 MPa
@Temperature -196 °C
 >= 395 MPa
@Thickness 177.8 - 203 mm
Hand forgings; short transverse
 >= 395 MPa
@Thickness 177.8 - 203 mm
Hand forgings; short transverse; T652
 >= 400 MPa
@Thickness 152.4 - 178 mm
Hand forgings; short transverse
 >= 400 MPa
@Thickness 152.4 - 178 mm
Hand forgings; short transverse; T652
 >= 405 MPa
@Thickness 76.23 - 102 mm
Plate; T62, T651
 >= 405 MPa
@Thickness 127.0 - 152 mm
Hand forgings; short transverse
 >= 405 MPa
@Thickness 177.8 - 203 mm
Hand forgings; longitudinal, long transverse
 >= 405 MPa
@Thickness 127.0 - 152 mm
Hand forgings; short transverse; T652
 >= 405 MPa
@Thickness 177.8 - 203 mm
Hand forgings; longitudinal, long transverse; T652
 >= 415 MPa
@Thickness <=12.7 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 >= 415 MPa
@Thickness <=12.7 mm
Extruded tube; T6, T6510, T6511
 >= 415 MPa
@Thickness 101.6 - 127 mm
Hand forgings; short transverse
 >= 415 MPa
@Thickness 152.4 - 178 mm
Hand forgings; longitudinal, long transverse
 >= 415 MPa
@Thickness 101.6 - 127 mm
Hand forgings; short transverse; T652
 >= 415 MPa
@Thickness 152.4 - 178 mm
Hand forgings; longitudinal, long transverse; T652
 >= 415 MPa
@Thickness <=63.5 mm
Rolled rings; T6, T652; Radial
 >= 420 MPa
@Thickness 76.23 - 102 mm
Hand forgings; short transverse
 >= 420 MPa
@Thickness 127.0 - 152 mm
Hand forgings; longitudinal, long transverse
 >= 420 MPa
@Thickness 76.23 - 102 mm
Hand forgings; short transverse; T652
 >= 420 MPa
@Thickness 127.0 - 152 mm
Hand forgings; longitudinal, long transverse; T652
 >= 425 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; short transverse
 >= 425 MPa
@Thickness 101.6 - 127 mm
Hand forgings; longitudinal, long transverse
 >= 425 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; short transverse; T652
 >= 425 MPa
@Thickness 101.6 - 127 mm
Hand forgings; longitudinal, long transverse; T652
 >= 425 MPa
@Thickness <=63.5 mm
Rolled rings; T6, T652; Axial
 >= 425 MPa
@Thickness 63.53 - 76.2 mm
Rolled rings; T6, T652; Axial
 >= 435 MPa
@Thickness 63.53 - 76.2 mm
Plate; T62, T651
 >= 435 MPa
@Thickness 76.2 - 102 mm
Die forgings: axis parallel to direction of grain flow
 >= 435 MPa
@Thickness 50.8 - 102 mm
Die forgings: axis not parallel to direction of grain flow
 >= 435 MPa
@Thickness 76.23 - 102 mm
Hand forgings; longitudinal, long transverse
 >= 435 MPa
@Thickness 76.23 - 102 mm
Hand forgings; longitudinal, long transverse; T652
 >= 440 MPa
@Thickness 0.508 - 0.991 mm
Sheet; T6, T62
 >= 440 MPa
@Thickness 12.7 - 19.0 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 >= 440 MPa
@Thickness 12.7 - 19.0 mm
Extruded tube; T6, T6510, T6511
 >= 440 MPa
@Thickness <=50.8 mm
Die forgings: axis not parallel to direction of grain flow
 >= 440 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; longitudinal
 >= 440 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; long transverse
 >= 440 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; longitudinal; T652
 >= 440 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; long transverse; T652
 >= 450 MPa
@Thickness 50.83 - 63.5 mm
Plate; T62, T651
 >= 450 MPa
@Thickness <=50.8 mm
Die forgings: axis parallel to direction of grain flow
 >= 450 MPa
@Thickness 50.8 - 76.2 mm
Die forgings: axis parallel to direction of grain flow
 >= 450 MPa
@Thickness <=50.8 mm
Hand forgings; longitudinal, long transverse
 >= 450 MPa
@Thickness <=50.8 mm
Hand forgings; longitudinal, long transverse; T652
 >= 450 MPa
@Thickness <=63.5 mm
Rolled rings; T6, T652; Tangential
 >= 450 MPa
@Thickness 63.53 - 76.2 mm
Rolled rings; T6, T652; Tangential
 >= 455 MPa
@Thickness 1.02 - 6.32 mm
Sheet; T6, T62
 >= 460 MPa
@Thickness 6.35 - 50.8 mm
Plate; T62, T651
 >= 470 MPa
@Thickness >=19.0 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 >= 470 MPa
@Thickness >=19.0 mm
Extruded tube; T6, T6510, T6511
Tensile Strength, Yield 60.0 ksiAA; Typical
 >= 365 MPaExtruded tube; T62
 >= 365 MPaExtruded wire, rod, bar, and shapes; T62
 >= 380 MPaRolled or cold finished wire (rod and bar); T6, T62, T651
 >= 330 MPa
@Thickness 177.8 - 203 mm
Hand forgings; short transverse; T652
 >= 340 MPa
@Thickness 152.4 - 178 mm
Hand forgings; short transverse; T652
 >= 345 MPa
@Thickness 101.6 - 127 mm
Hand forgings; short transverse; T652
 >= 345 MPa
@Thickness 127.0 - 152 mm
Hand forgings; short transverse; T652
 >= 350 MPa
@Thickness 177.8 - 203 mm
Hand forgings; longitudinal, long transverse
 >= 350 MPa
@Thickness 177.8 - 203 mm
Hand forgings; short transverse
 >= 350 MPa
@Thickness 76.23 - 102 mm
Hand forgings; short transverse; T652
 >= 350 MPa
@Thickness 177.8 - 203 mm
Hand forgings; longitudinal, long transverse; T652
 >= 360 MPa
@Thickness 152.4 - 178 mm
Hand forgings; longitudinal, long transverse
 >= 360 MPa
@Thickness 152.4 - 178 mm
Hand forgings; short transverse
 >= 360 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; short transverse; T652
 >= 360 MPa
@Thickness 152.4 - 178 mm
Hand forgings; longitudinal, long transverse; T652
 >= 360 MPa
@Thickness <=63.5 mm
Rolled rings; T6, T652; Radial
 >= 360 MPa
@Thickness 63.53 - 76.2 mm
Rolled rings; T6, T652; Axial
 >= 365 MPa
@Thickness <=12.7 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 >= 365 MPa
@Thickness 101.6 - 127 mm
Hand forgings; short transverse
 >= 365 MPa
@Thickness 127.0 - 152 mm
Hand forgings; longitudinal, long transverse
 >= 365 MPa
@Thickness 127.0 - 152 mm
Hand forgings; short transverse
 >= 365 MPa
@Thickness 127.0 - 152 mm
Hand forgings; longitudinal, long transverse; T652
 >= 365 MPa
@Thickness <=12.7 mm
Extruded tube; T6, T6510, T6511
 >= 370 MPa
@Thickness 50.8 - 102 mm
Die forgings: axis not parallel to direction of grain flow
 >= 370 MPa
@Thickness 76.23 - 102 mm
Hand forgings; short transverse
 >= 370 MPa
@Thickness 101.6 - 127 mm
Hand forgings; longitudinal, long transverse
 >= 370 MPa
@Thickness 101.6 - 127 mm
Hand forgings; longitudinal, long transverse; T652
 >= 380 MPa
@Thickness 76.23 - 102 mm
Plate; T62, T651
 >= 380 MPa
@Thickness 76.2 - 102 mm
Die forgings: axis parallel to direction of grain flow
 >= 380 MPa
@Thickness <=50.8 mm
Die forgings: axis not parallel to direction of grain flow
 >= 380 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; long transverse
 >= 380 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; short transverse
 >= 380 MPa
@Thickness 76.23 - 102 mm
Hand forgings; longitudinal, long transverse
 >= 380 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; long transverse; T652
 >= 380 MPa
@Thickness 76.23 - 102 mm
Hand forgings; longitudinal, long transverse; T652
 >= 380 MPa
@Thickness <=63.5 mm
Rolled rings; T6, T652; Tangential
 >= 380 MPa
@Thickness <=63.5 mm
Rolled rings; T6, T652; Axial
 >= 380 MPa
@Thickness 63.53 - 76.2 mm
Rolled rings; T6, T652; Tangential
 >= 380 MPa
@Thickness 50.8 - 76.2 mm
Die forgings: axis parallel to direction of grain flow
 >= 385 MPa
@Thickness <=50.8 mm
Die forgings: axis parallel to direction of grain flow
 >= 385 MPa
@Thickness <=50.8 mm
Hand forgings; longitudinal, long transverse
 >= 385 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; longitudinal
 >= 385 MPa
@Thickness <=50.8 mm
Hand forgings; longitudinal, long transverse; T652
 >= 385 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; longitudinal; T652
 >= 395 MPa
@Thickness 0.508 - 0.991 mm
Sheet; T6, T62
 >= 395 MPa
@Thickness 63.53 - 76.2 mm
Plate; T62, T651
 >= 400 MPa
@Thickness 1.02 - 6.32 mm
Sheet; T6, T62
 >= 400 MPa
@Thickness 50.83 - 63.5 mm
Plate; T62, T651
 >= 400 MPa
@Thickness 12.7 - 19.0 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 >= 400 MPa
@Thickness 12.7 - 19.0 mm
Extruded tube; T6, T6510, T6511
 >= 405 MPa
@Thickness 6.35 - 50.8 mm
Plate; T62, T651
 >= 415 MPa
@Thickness >=19.0 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 >= 415 MPa
@Thickness >=19.0 mm
Extruded tube; T6, T6510, T6511
 24.0 MPa
@Strain 0.2 %,
Temperature 371 °C
 34.0 MPa
@Strain 0.2 %,
Temperature 316 °C
 52.0 MPa
@Strain 0.2 %,
Temperature 260 °C
 90.0 MPa
@Strain 0.2 %,
Temperature 204 °C
 241 MPa
@Strain 0.2 %,
Temperature 149 °C
 393 MPa
@Strain 0.2 %,
Temperature 100 °C
 414 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 427 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 448 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 496 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 7.0 %Extruded tube; T62
 7.0 %Extruded wire, rod, bar, and shapes; T62
 8.0 %Rolled or cold finished wire (rod and bar); T6, T62, T651
 13 %
@Temperature -28.0 °C
 13 %
@Temperature 24.0 °C
 13 %
@Temperature -80.0 °C
 14 %
@Temperature -196 °C
 15 %
@Temperature 100 °C
 20 %
@Temperature 149 °C
 38 %
@Temperature 204 °C
 52 %
@Temperature 260 °C
 65 %
@Temperature 316 °C
 72 %
@Temperature 371 °C
 1.0 %
@Thickness 76.23 - 102 mm
Plate; T62, T651
 1.0 %
@Thickness 101.6 - 127 mm
Hand forgings; short transverse
 1.0 %
@Thickness 127.0 - 152 mm
Hand forgings; short transverse
 1.0 %
@Thickness 152.4 - 178 mm
Hand forgings; short transverse
 1.0 %
@Thickness 177.8 - 203 mm
Hand forgings; short transverse
 1.0 %
@Thickness 101.6 - 127 mm
Hand forgings; short transverse; T652
 1.0 %
@Thickness 127.0 - 152 mm
Hand forgings; short transverse; T652
 1.0 %
@Thickness 152.4 - 178 mm
Hand forgings; short transverse; T652
 1.0 %
@Thickness 177.8 - 203 mm
Hand forgings; short transverse; T652
 2.0 %
@Thickness 50.83 - 63.5 mm
Plate; T62, T651
 2.0 %
@Thickness 63.53 - 76.2 mm
Plate; T62, T651
 2.0 %
@Thickness 63.53 - 76.2 mm
Rolled rings; T6, T652; Axial
 2.0 %
@Thickness 50.8 - 102 mm
Die forgings: axis not parallel to direction of grain flow
 2.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; short transverse
 2.0 %
@Thickness 76.23 - 102 mm
Hand forgings; short transverse
 2.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; short transverse; T652
 2.0 %
@Thickness 76.23 - 102 mm
Hand forgings; short transverse; T652
 2.0 %
@Thickness <=63.5 mm
Rolled rings; T6, T652; Radial
 3.0 %
@Thickness <=50.8 mm
Die forgings: axis not parallel to direction of grain flow
 3.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; long transverse
 3.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; long transverse; T652
 3.0 %
@Thickness <=63.5 mm
Rolled rings; T6, T652; Axial
 2.0 - 6.0 %
@Thickness 152.4 - 178 mm
Hand forgings; longitudinal, long transverse; T652
 2.0 - 6.0 %
@Thickness 177.8 - 203 mm
Hand forgings; longitudinal, long transverse; T652
 2.0 - 7.0 %
@Thickness 101.6 - 127 mm
Hand forgings; longitudinal, long transverse
 2.0 - 7.0 %
@Thickness 127.0 - 152 mm
Hand forgings; longitudinal, long transverse
 2.0 - 7.0 %
@Thickness 152.4 - 178 mm
Hand forgings; longitudinal, long transverse
 2.0 - 7.0 %
@Thickness 177.8 - 203 mm
Hand forgings; longitudinal, long transverse
 2.0 - 7.0 %
@Thickness 101.6 - 127 mm
Hand forgings; longitudinal, long transverse; T652
 2.0 - 7.0 %
@Thickness 127.0 - 152 mm
Hand forgings; longitudinal, long transverse; T652
 3.0 - 8.0 %
@Thickness <=50.8 mm
Hand forgings; longitudinal, long transverse
 3.0 - 8.0 %
@Thickness 76.23 - 102 mm
Hand forgings; longitudinal, long transverse
 3.0 - 8.0 %
@Thickness <=50.8 mm
Hand forgings; longitudinal, long transverse; T652
 3.0 - 8.0 %
@Thickness 76.23 - 102 mm
Hand forgings; longitudinal, long transverse; T652
 4.0 - 7.0 %
@Thickness 6.35 - 50.8 mm
Plate; T62, T651
 6.0 %
@Thickness 0.508 - 0.991 mm
Sheet; T6, T62
 6.0 %
@Thickness <=50.8 mm
Die forgings: axis parallel to direction of grain flow
 6.0 %
@Thickness 50.8 - 76.2 mm
Die forgings: axis parallel to direction of grain flow
 6.0 %
@Thickness 76.2 - 102 mm
Die forgings: axis parallel to direction of grain flow
 6.0 %
@Thickness 63.53 - 76.2 mm
Rolled rings; T6, T652; Tangential
 7.0 %
@Thickness 1.02 - 6.32 mm
Sheet; T6, T62
 7.0 %
@Thickness <=12.7 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 7.0 %
@Thickness 12.7 - 19.0 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 7.0 %
@Thickness >=19.0 mm
Extruded wire, rod, bar, and shapes; T6, T6510, T6511
 7.0 %
@Thickness <=63.5 mm
Rolled rings; T6, T652; Tangential
 7.0 %
@Thickness <=12.7 mm
Extruded tube; T6, T6510, T6511
 7.0 %
@Thickness 12.7 - 19.0 mm
Extruded tube; T6, T6510, T6511
 7.0 %
@Thickness >=19.0 mm
Extruded tube; T6, T6510, T6511
 8.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; longitudinal
 8.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; longitudinal; T652
 13 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Tensile Modulus 72.4 GPa
Compressive Strength 470 MPa
Compressive Modulus 73.8 GPa
Notched Tensile Strength 414 MPa2.5 cm width x 0.16 cm thick side-notched specimen, Kt = 17.
Ultimate Bearing Strength 889 MPaEdge distance/pin diameter = 2.0
Bearing Yield Strength 662 MPaEdge distance/pin diameter = 2.0
Poissons Ratio 0.33
Fatigue Strength 18000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Fracture Toughness 19.0 MPa-m½KIC; TL orientation.
Machinability 70 %0-100 Scale of Aluminum Alloys
Shear Modulus 28.0 GPa
Shear Strength 42.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 26.0 ohm-cir-mil/ft
@Temperature 20.0 °C
AA; Typical
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.8 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
average
Specific Heat Capacity 0.880 J/g-°CEstimated from trends in similar Al alloys.
Thermal Conductivity 1070 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 945 - 1180 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 945 °FAA; Typical
Liquidus 1180 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 935 °F
Aging Temperature 320 °FSheet, plate, wire, rod, bar, shapes, tube; 18 hr at temperature
 340 °FForgings; 10 hr at temperature
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 90.4 - 95 %As remainder
Chromium, Cr <= 0.10 %
Copper, Cu 3.9 - 5.0 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.20 - 0.80 %
Manganese, Mn 0.40 - 1.2 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.50 - 1.2 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2014-T6; 2014-T651
DWA 6092/SiC/17.5p-T6 Aluminum SiC Metal-Matrix-Composite (Al MMC), Sheet
Aluminum 2014-T4; 2014-T451
Alclad Aluminum 2014-T6, T651
Aluminum 2014-O

MA2014T6a / 171250

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.