MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

(Viewing data as-entered. Click here to return)
Tra-Con Tra-Duct 2902 Room Temperature Conductive Silver Epoxy Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy, Electrically Conductive; Filled/Reinforced Thermoset

Material Notes: TRA-DUCT 2902 is an electrically conducting silver-filled epoxy compound recommended for electronic bonding and sealing applications that require a combination of good mechanical and electrical properties. This two-part, smooth paste formulation of refined pure silver and epoxy is free of solvents and copper or carbon additives. It develops strong, durable, electrically and thermally conducting bonds and coatings between many different and dissimilar materials such as metals, ceramics, glass and plastic laminates. TRA-DUCT 2902 cures at room temperature and can be used as a cold solder for heat-sensitive components where hot-soldering is impractical. It also can be used for the assembly and repair of electrical modules, printed circuits, wave guides, flat cables and high frequency shields. This adhesive complies with the requirements of NASA Outgassing Specification.

Information provided by Tra-Con Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 3.20 g/ccMixed
Viscosity 20000 cPMixed (cp #52, 10 rpm)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 80
Adhesive Bond Strength 700 psiLap shear, alum to alum, 24 hrs @ 25°C
 1000 psiLap shear, alum to alum, 2 hrs @ 65°C
 1600 psiLap shear, alum to alum, 1 hr @ 110°C
 1600 psiLap shear, alum to alum, 15 min @ 150°C
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 0.00030 ohm-cmcured 5 min @ 160°C
 0.00050 ohm-cmcured 15 min @ 150°C
 0.00060 ohm-cmcured 1 hr @ 110°C
 0.00090 ohm-cmcured 2 hrs @ 65°C
 0.0010 ohm-cmcured 24 hrs @ 25°C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 49.0 µm/m-°C
@Temperature 20.0 °C
Thermal Conductivity 2.99 W/m-K
Maximum Service Temperature, Air 110 °C
Minimum Service Temperature, Air -60.0 °C
Glass Transition Temp, Tg 52.0 °CUltimate Tg, 24 hrs @ 25°C
 
Processing PropertiesOriginal ValueComments
Cure Time 1.00 - 4.00 hour
@Temperature 65.0 °C
 24.0 hour
@Temperature 25.0 °C
Pot Life 60 min
 
Descriptive Properties
Color Silver
Cytotoxicity Study PassesISO 10993-5, elution method
Mix Ratio, parts by weight100/6Resin/Hardener
Outgassing, NASA Passes
Outgassing, NASA, %CVCM0.05

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Abatron 8602-2 A/B Carbon-Filled Electrically Conductive Epoxy Compound
Tra-Con Tra-Bond 293-14 Electrically Conductive Silver-Filled Epoxy Adhesive
Tra-Con Tra-Duct 2960 Snap Cure Electrically Conductive Silver-Filled Epoxy
Tra-Con Tra-Duct 916H01 Electronically Conductive Silver-Filled Epoxy
Tra-Con Tra-Duct 8205 One-Part Electrically Conductive Silver-Filled Epoxy

PTRAC077 / 71005

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.