MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Eastman Eastar CN005 Copolyester, High Flow Grade
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Applications:
  • Compacts
  • Cosmetic jar caps
  • Cosmetic jars
  • Cosmetics/personal care packaging
  • Fragrance caps
  • Fragrance packaging
  • Lip gloss containers
  • Lipstick containers
  • Personal care bottles

Key Attributes:

  • Ability to mold thick parts
  • Ease of processing
  • Easy to extrude, cut, decorate and seal
  • Excellent chemical resistance
  • Excellent clarity and color
  • Excellent colorability
  • Good impact strength
  • Good stiffness
  • High gloss appearance
  • Improved gate aesthetics
  • Readily fill intricate molds
  • Toughness

Product Description: Eastar CN005 copolyester is a high flow product. It is the first copolyester resin from Eastman that has been designed and engineered specifically for cosmetics packaging applications. With its great color and clarity and ability to mold thick parts with improved gate aesthetics, Eastar CN is clearly the most suited copolyester for premium cosmetics packaging. Other features of Eastar CN are excellent chemical resistance, high gloss, and improvements in processing such as faster drying times, faster cycle times, and lower scrap rates. Eastar CN is also ideally suited for two-shot molding techniques due to its lower processing temperatures, very slow crystallization rate, and flow characteristics. This product has been GREENGUARD INDOOR AIR QUALITY CERTIFIED®.

Information provided by Eastman.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.20 g/ccASTM D792
Linear Mold Shrinkage 0.0030 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 105ASTM D785
Tensile Strength at Break 35.0 MPaASTM D638
Tensile Strength, Yield 50.0 MPaASTM D638
Elongation at Break 193 %ASTM D638
Elongation at Yield 4.5 %ASTM D638
Flexural Strength 67.0 MPaASTM D790
Flexural Modulus 1800 MPaASTM D790
Izod Impact, Notched 38.0 J/m
@Temperature -40.0 °C
ASTM D256
 70.0 J/m
@Temperature 23.0 °C
ASTM D256
Izod Impact, Unnotched NB
@Temperature 23.0 °C
ASTM D4812
 NB
@Temperature -40.0 °C
ASTM D4812
Puncture Energy 40.0 JAt Max load; ASTM D3763
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 71.0 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 63.0 °CASTM D648
 
Optical PropertiesOriginal ValueComments
Haze <= 0.60 %ASTM D1003
Transmission, Visible 90 %Total; ASTM D1003
 
Processing PropertiesOriginal ValueComments
Melt Temperature 205 - 240 °C
Mold Temperature 16.0 - 50.0 °C
Drying Temperature 50.0 °C
Dry Time 2 - 4 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Eastman Eastar EN067 Copolyester, Natural
Eastman AP005 Copolyester
Overview of materials for PETG Copolyester
3M FL012 Lexan Label Product
Avient Edgetek® COC BLEND-15GF Natural Cyclic Olefin Copolymer (COC)

PE8804 / 129649

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.