MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2219-T851
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92219; ISO AlCu6Mn; Aluminium 2219-T851; AA2219-T851; Al2219-T851
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.84 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 130500 kg load with 10 mm ball
Hardness, Knoop 163Converted from Brinell Hardness Value
Hardness, Rockwell A 49.5Converted from Brinell Hardness Value
Hardness, Rockwell B 80Converted from Brinell Hardness Value
Hardness, Vickers 149Converted from Brinell Hardness Value
Tensile Strength, Ultimate 66.0 ksiAA; Typical
 >= 400 MPaWire, rod, bar, and shapes (extruded); T8510, T8511
 >= 400 MPaExtruded tube; T8510, T8511
 30.0 MPa
@Temperature 371 °C
 48.0 MPa
@Temperature 316 °C
 200 MPa
@Temperature 260 °C
 248 MPa
@Temperature 204 °C
 338 MPa
@Temperature 149 °C
 414 MPa
@Temperature 100 °C
 455 MPa
@Temperature 24.0 °C
 476 MPa
@Temperature -28.0 °C
 490 MPa
@Temperature -80.0 °C
 572 MPa
@Temperature -196 °C
 >= 395 MPa
@Thickness 127.0 - 152 mm
Plate
 >= 405 MPa
@Thickness 101.6 - 127 mm
Plate
 >= 415 MPa
@Thickness 76.23 - 102 mm
Plate
 >= 425 MPa
@Thickness 6.35 - 50.8 mm
Plate
 >= 425 MPa
@Thickness 50.83 - 76.2 mm
Plate
 >= 395 MPa
@Diameter 50.83 - 102 mm
Wire, rod, and bar (rolled or cold finished)
 >= 400 MPa
@Diameter 12.7 - 50.8 mm
Wire, rod, and bar (rolled or cold finished)
Tensile Strength, Yield 51.0 ksiAA; Typical
 >= 290 MPaWire, rod, bar, and shapes (extruded); T8510, T8511
 >= 290 MPaExtruded tube; T8510, T8511
 >= 290 MPa
@Thickness 127.0 - 152 mm
Plate
 >= 295 MPa
@Thickness 101.6 - 127 mm
Plate
 >= 305 MPa
@Thickness 76.23 - 102 mm
Plate
 >= 310 MPa
@Thickness 50.83 - 76.2 mm
Plate
 >= 315 MPa
@Thickness 6.35 - 50.8 mm
Plate
 >= 270 MPa
@Diameter 50.83 - 102 mm
Wire, rod, and bar (rolled or cold finished)
 >= 275 MPa
@Diameter 12.7 - 50.8 mm
Wire, rod, and bar (rolled or cold finished)
 26.0 MPa
@Strain 0.2 %,
Temperature 371 °C
 41.0 MPa
@Strain 0.2 %,
Temperature 316 °C
 159 MPa
@Strain 0.2 %,
Temperature 260 °C
 200 MPa
@Strain 0.2 %,
Temperature 204 °C
 276 MPa
@Strain 0.2 %,
Temperature 149 °C
 324 MPa
@Strain 0.2 %,
Temperature 100 °C
 345 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 359 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 372 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 421 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 6.0 %Wire, rod, bar, and shapes (extruded); T8510, T8511
 6.0 %Extruded tube; T8510, T8511
 12 %
@Temperature -28.0 °C
 12 %
@Temperature 24.0 °C
 13 %
@Temperature -80.0 °C
 15 %
@Temperature -196 °C
 15 %
@Temperature 100 °C
 17 %
@Temperature 149 °C
 20 %
@Temperature 204 °C
 21 %
@Temperature 260 °C
 55 %
@Temperature 316 °C
 75 %
@Temperature 371 °C
 4.0 %
@Thickness 127.0 - 152 mm
Plate
 5.0 %
@Thickness 76.23 - 102 mm
Plate
 5.0 %
@Thickness 101.6 - 127 mm
Plate
 6.0 %
@Thickness 50.83 - 76.2 mm
Plate
 7.0 - 8.0 %
@Thickness 6.35 - 50.8 mm
Plate
 10 %
@Thickness 1.59 mm
AA; Typical
 4.0 %
@Diameter 12.7 - 50.8 mm
Wire, rod, and bar (rolled or cold finished)
 4.0 %
@Diameter 50.83 - 102 mm
Wire, rod, and bar (rolled or cold finished)
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 15000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPaEstimated from similar Al alloys.
Shear Strength 285 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000570 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.864 J/g-°C
Thermal Conductivity 120 W/m-K
Melting Point 1010 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 1010 °FAA; Typical
Liquidus 1190 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 995 °F
Aging Temperature 325 - 375 °Ffrom 18 to 36 hr at temperature
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 91.5 - 93.8 %As remainder
Copper, Cu 5.8 - 6.8 %
Iron, Fe <= 0.30 %
Magnesium, Mg <= 0.02 %
Manganese, Mn 0.20 - 0.40 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.20 %
Titanium, Ti 0.02 - 0.10 %
Vanadium, V 0.05 - 0.15 %
Zinc, Zn <= 0.10 %
Zirconium, Zr 0.10 - 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2219-T351
Aluminum 2219-T62
Aluminum 2219-T81
Aluminum 2219-T6
Aluminum 2219-T851 (Extended High Temperature Data)

MA2219T851 / 8934

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.