MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Huntsman IROGRAN® D 64 P 4777 TPU-Polyester
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyester Grade

Material Notes: Polyether-based grades for film and sheet applications that require excellent resistance to hydrolysis and microbial attack.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.17 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 95ASTM D2240
Hardness, Shore D 65ASTM D2240
Tensile Strength at Break 6110 psiASTM D412
Elongation at Break 380 %ASTM D412
50% Modulus 2.68 ksi
@Strain 50 %
ASTM D412
100% Modulus 3.07 ksi
@Strain 100 %
ASTM D412
300% Modulus 4.91 ksi
@Strain 300 %
ASTM D412
Rebound 50 %Bayshore; ASTM D2632
Tear Strength 950 pliASTM D624
Taber Abrasion, mg/1000 Cycles 77ASTM D3389
Abrasion 48mm3; DIN 53516
Compression Set 57 %
@Temperature 22.8 °C,
Time 79200 sec
ASTM D395
 92 %
@Temperature 70.0 °C,
Time 79200 sec
ASTM D395
 
Thermal PropertiesOriginal ValueComments
Melting Point 188 - 204 °CTMA Melt Range
Vicat Softening Point 137 °CASTM D1525
Glass Transition Temp, Tg -41.0 °CMidpoint; ASTM E 1269

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Huntsman AVALON® 60 DB Thermoplastic Polyurethane
Huntsman IROGRAN® D 60 E 4024 Polyester-Based TPU-High Performance Grade
Huntsman IROGRAN® PS 370-202 TPU-Polyester
Huntsman IROGRAN® A 85 E 4607 E TPU-Polyester
Huntsman IROGRAN® A 95 K 4640 TPU-For Seals

PHUQ119 / 159492

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.