MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
RTP Company Permaprene™ 2800 B-65A Thermoplastic Polyolefin Elastomer (TEO)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Olefinic TPE

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.02 g/ccASTM D 792
Linear Mold Shrinkage 0.012 - 0.018 cm/cm
@Thickness 3.20 mm
ASTM D 955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 6810 s delay; ASTM D 2240
Tensile Strength at Break 800 psiDie C, 0.125 in (3.2mm); 20 in/min (500 mm/min); ASTM D 412
Tensile Strength, Yield 350 psiDie C 0.125 in (3.2 mm); 20 in/min (500 mm/min); 100%; ASTM D 412
Elongation at Break 500 %Die C, 0.125 in (3.2mm); 20 in/min (500 mm/min); ASTM D 412
Tear Strength 145 pliDie C; ASTM D 624
Compression Set 22 %
@Temperature 23.0 °C,
Time 79200 sec
Method B; Type 2; ASTM D 395
 36 %
@Temperature 70.0 °C,
Time 79200 sec
Method B; Type 2; ASTM D 395
 
Processing PropertiesOriginal ValueComments
Melt Temperature 360 - 410 °F
Mold Temperature 60.0 - 150 °F
Drying Temperature 175 °F
@Time 7200 sec
Moisture Content <= 0.050 %
Dew Point 0.000 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow INFUSE™ 9817 Olefin Block Copolymer
A. Schulman POLYTROPE™ TPP 530 Injection Molding Grade Olefinic Thermoplastic Elastomer
Noble Polymers Regis™ 315107 Thermoplastic Olefin (TPO)
A. Schulman POLYTROPE™ TPP 620 Olefinic Elastomer
Avient Elastamax™ XL-2055 Thermoplastic Polyolefin Elastomer (TPO (POE))

PQZRA37542 / 206142

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.