MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI 1141 Steel, normalized at 900°C (1650°F), air cooled, round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Medium Carbon Steel

Material Notes: Applications include cold drawn or finished bar, cold punched nuts, split rivets, machine screws, and wood screws.

Key Words: UNS G11410, ASTM A29, ASTM A107, ASTM A108, ASTM A311, FED QQ-S-637, SAE J403, SAE J412, SAE J414
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.87 g/cc0.284 lb/in³Typical for steel.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  201
@Diameter 25.4 mm
201
@Diameter 1.00 in
 201
@Diameter 50.8 mm
201
@Diameter 2.00 in
 201
@Diameter 102 mm
201
@Diameter 4.00 in
 207
@Diameter 12.7 mm
207
@Diameter 0.500 in
Hardness, Knoop  223
@Diameter 25.4 mm
223
@Diameter 1.00 in
Converted from Brinell
 223
@Diameter 50.8 mm
223
@Diameter 2.00 in
Converted from Brinell
 223
@Diameter 102 mm
223
@Diameter 4.00 in
Converted from Brinell
 229
@Diameter 12.7 mm
229
@Diameter 0.500 in
Converted from Brinell
Hardness, Rockwell B  93
@Diameter 12.7 mm
93
@Diameter 0.500 in
Converted from Brinell
 93
@Diameter 25.4 mm
93
@Diameter 1.00 in
Converted from Brinell
 93
@Diameter 50.8 mm
93
@Diameter 2.00 in
Converted from Brinell
 93
@Diameter 102 mm
93
@Diameter 4.00 in
Converted from Brinell
Hardness, Rockwell C  13
@Diameter 25.4 mm
13
@Diameter 1.00 in
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
 13
@Diameter 50.8 mm
13
@Diameter 2.00 in
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
 13
@Diameter 102 mm
13
@Diameter 4.00 in
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
 15
@Diameter 12.7 mm
15
@Diameter 0.500 in
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
Hardness, Vickers  211
@Diameter 25.4 mm
211
@Diameter 1.00 in
Converted from Brinell
 211
@Diameter 50.8 mm
211
@Diameter 2.00 in
Converted from Brinell
 211
@Diameter 102 mm
211
@Diameter 4.00 in
Converted from Brinell
 217
@Diameter 12.7 mm
217
@Diameter 0.500 in
Converted from Brinell
Tensile Strength, Ultimate  689 MPa
@Diameter 102 mm
99900 psi
@Diameter 4.00 in
 696 MPa
@Diameter 50.8 mm
101000 psi
@Diameter 2.00 in
 703 MPa
@Diameter 25.4 mm
102000 psi
@Diameter 1.00 in
 731 MPa
@Diameter 12.7 mm
106000 psi
@Diameter 0.500 in
Tensile Strength, Yield  380 MPa
@Diameter 102 mm
55100 psi
@Diameter 4.00 in
 395 MPa
@Diameter 50.8 mm
57300 psi
@Diameter 2.00 in
 405 MPa
@Diameter 25.4 mm
58700 psi
@Diameter 1.00 in
 425 MPa
@Diameter 12.7 mm
61600 psi
@Diameter 0.500 in
Elongation at Break  21.7 %
@Diameter 102 mm
21.7 %
@Diameter 4.00 in
 22.5 %
@Diameter 50.8 mm
22.5 %
@Diameter 2.00 in
 22.7 %
@Diameter 12.7 mm
22.7 %
@Diameter 0.500 in
 22.7 %
@Diameter 25.4 mm
22.7 %
@Diameter 1.00 in
Reduction of Area  49.3 %
@Diameter 102 mm
49.3 %
@Diameter 4.00 in
 55.5 %
@Diameter 25.4 mm
55.5 %
@Diameter 1.00 in
 55.8 %
@Diameter 50.8 mm
55.8 %
@Diameter 2.00 in
 57.8 %
@Diameter 12.7 mm
57.8 %
@Diameter 0.500 in
Modulus of Elasticity 200 GPa29000 ksiTypical for steel
Bulk Modulus 160 GPa23200 ksiTypical for steel.
Poissons Ratio 0.290.29Typical For Steel
Shear Modulus 80.0 GPa11600 ksiTypical for steel.
Izod Impact 53.0 J39.1 ft-lbnormalized at 900°C (1650°F)
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000170 ohm-cm
@Temperature 20.0 °C
0.0000170 ohm-cm
@Temperature 68.0 °F
condition of specimen unknown
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.5 µm/m-°C
@Temperature 20.0 °C
6.39 µin/in-°F
@Temperature 68.0 °F
Typical steel
 12.2 µm/m-°C
@Temperature 0.000 - 300 °C
6.78 µin/in-°F
@Temperature 32.0 - 572 °F
Typical for steel
 13.9 µm/m-°C
@Temperature 0.000 - 500 °C
7.72 µin/in-°F
@Temperature 32.0 - 932 °F
Typical for steel
Specific Heat Capacity 0.472 J/g-°C0.113 BTU/lb-°FTypical steel
Thermal Conductivity 51.9 W/m-K360 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.37 - 0.45 %0.37 - 0.45 %
Iron, Fe 97.73 - 98.2 %97.73 - 98.2 %As remainder
Manganese, Mn 1.35 - 1.65 %1.35 - 1.65 %
Phosphorus, P <= 0.040 %<= 0.040 %
Sulfur, S 0.080 - 0.13 %0.080 - 0.13 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 1141 Steel, normalized at 900°C (1650°F)
AISI 1141 Steel, oil quenched from 815°C, 540°C (1000°F) temper, 13 mm (0.5 in.) round
AISI 1045 Steel, Quenched and Tempered to 390 HB
AISI 1141 Steel, annealed at 815°C, furnace cooled 11°C (20°F) per hour to 480°C, cooled in air, 25 mm (1 in.) round
AISI 1141 Steel, as rolled

M114AT / 7253

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.