MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI 1141 Steel, normalized at 900°C (1650°F), air cooled, round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Medium Carbon Steel

Material Notes: Applications include cold drawn or finished bar, cold punched nuts, split rivets, machine screws, and wood screws.

Key Words: UNS G11410, ASTM A29, ASTM A107, ASTM A108, ASTM A311, FED QQ-S-637, SAE J403, SAE J412, SAE J414
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.87 g/ccTypical for steel.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 201
@Diameter 25.4 mm
 201
@Diameter 50.8 mm
 201
@Diameter 102 mm
 207
@Diameter 12.7 mm
Hardness, Knoop 223
@Diameter 25.4 mm
Converted from Brinell
 223
@Diameter 50.8 mm
Converted from Brinell
 223
@Diameter 102 mm
Converted from Brinell
 229
@Diameter 12.7 mm
Converted from Brinell
Hardness, Rockwell B 93
@Diameter 12.7 mm
Converted from Brinell
 93
@Diameter 25.4 mm
Converted from Brinell
 93
@Diameter 50.8 mm
Converted from Brinell
 93
@Diameter 102 mm
Converted from Brinell
Hardness, Rockwell C 13
@Diameter 25.4 mm
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
 13
@Diameter 50.8 mm
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
 13
@Diameter 102 mm
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
 15
@Diameter 12.7 mm
Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
Hardness, Vickers 211
@Diameter 25.4 mm
Converted from Brinell
 211
@Diameter 50.8 mm
Converted from Brinell
 211
@Diameter 102 mm
Converted from Brinell
 217
@Diameter 12.7 mm
Converted from Brinell
Tensile Strength, Ultimate 689 MPa
@Diameter 102 mm
 696 MPa
@Diameter 50.8 mm
 703 MPa
@Diameter 25.4 mm
 731 MPa
@Diameter 12.7 mm
Tensile Strength, Yield 380 MPa
@Diameter 102 mm
 395 MPa
@Diameter 50.8 mm
 405 MPa
@Diameter 25.4 mm
 425 MPa
@Diameter 12.7 mm
Elongation at Break 21.7 %
@Diameter 102 mm
 22.5 %
@Diameter 50.8 mm
 22.7 %
@Diameter 12.7 mm
 22.7 %
@Diameter 25.4 mm
Reduction of Area 49.3 %
@Diameter 102 mm
 55.5 %
@Diameter 25.4 mm
 55.8 %
@Diameter 50.8 mm
 57.8 %
@Diameter 12.7 mm
Modulus of Elasticity 200 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steel.
Poissons Ratio 0.29Typical For Steel
Shear Modulus 80.0 GPaTypical for steel.
Izod Impact 53.0 Jnormalized at 900°C (1650°F)
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000170 ohm-cm
@Temperature 20.0 °C
condition of specimen unknown
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.5 µm/m-°C
@Temperature 20.0 °C
Typical steel
 12.2 µm/m-°C
@Temperature 0.000 - 300 °C
Typical for steel
 13.9 µm/m-°C
@Temperature 0.000 - 500 °C
Typical for steel
Specific Heat Capacity 0.472 J/g-°CTypical steel
Thermal Conductivity 51.9 W/m-KTypical steel
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.37 - 0.45 %
Iron, Fe 97.73 - 98.2 %As remainder
Manganese, Mn 1.35 - 1.65 %
Phosphorus, P <= 0.040 %
Sulfur, S 0.080 - 0.13 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1141 Steel, normalized at 900°C (1650°F)
AISI 1141 Steel, oil quenched from 815°C, 540°C (1000°F) temper, 13 mm (0.5 in.) round
AISI 1045 Steel, Quenched and Tempered to 390 HB
AISI 1141 Steel, annealed at 815°C, furnace cooled 11°C (20°F) per hour to 480°C, cooled in air, 25 mm (1 in.) round
AISI 1141 Steel, as rolled

M114AT / 7253

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.