MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Durethan® BKV 30 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled

Material Notes: PA 6, 30% glass fibers, injection molding

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.700 g/ccISO 60
Density 1.36 g/ccISO 1183
Moisture Absorption at Equilibrium 2.1 %50% RH; ISO 62
Water Absorption at Saturation 7.0 %IOS 62
Linear Mold Shrinkage, Flow 0.0016 cm/cm150x105x3; 280 °C / MT 80 °C; 500 bar; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0082 cm/cm150x105x3; 280 °C / MT 80 °C; 500 bar; ISO 294-4
Melt Flow 14 g/10 min
@Load 5.00 kg,
Temperature 260 °C
ISO 1133-1
 
Mechanical PropertiesOriginal ValueComments
Puncture Resistance 950 N
@Temperature -30.0 °C
ISO 6603-2
 1071 N
@Temperature 23.0 °C
ISO 6603-2
Ball Indentation Hardness 210 MPaISO 2093-1
Tensile Strength at Break 180 MPa5 mm/min; ISO 527-1,-2
Elongation at Break 3.0 %5 mm/min; ISO 527-1,-2
Tensile Modulus 9800 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 280 MPa2 mm/min; ISO 178-A
Flexural Modulus 8600 MPa2 mm/min; ISO 178-A
Flexural Strain at Break 4.0 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO) 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
 15.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
Izod Impact, Unnotched (ISO) 60.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1U
 75.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
Charpy Impact Unnotched 70.0 kJ/m²
@Temperature -30.0 °C
ISO 179-1eU
 80.0 kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
Charpy Impact, Notched 10.0 kJ/m²
@Temperature -30.0 °C
ISO 179 1eA
 15.0 kJ/m²
@Temperature 23.0 °C
ISO 179 1eA
Puncture Energy 6.00 J
@Temperature -30.0 °C
ISO 6603-2
 8.00 J
@Temperature 23.0 °C
ISO 6603-2
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+14 ohmIEC 60093
Dielectric Constant 4.0
@Frequency 100 Hz
IEC 60250
 4.0
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 40.0 kV/mm
@Thickness 1.00 mm
IEC 60243-1
Dissipation Factor 0.0050
@Frequency 100 Hz
IEC 60250
 0.015
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 400 VSolution B; IEC 60112
 600 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 20.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
CTE, linear, Transverse to Flow 80.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Melting Point 222 °C10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi) 215 °CISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 200 °CISO 75-1,-2
Vicat Softening Point >= 200 °C
@Load 5.10 kg
120°C/h; ISO 306
 >= 200 °C
@Load 5.10 kg
50°C/h; ISO 306
Flammability, UL94 HB
@Thickness 1.60 mm
 HB
@Thickness 3.20 mm
Oxygen Index 22 %Method A; ISO 4589-2
Glow Wire Flammability Index 600 °C
@Thickness 2.00 mm
IEC 60695-2-12
Shrinkage, MD 0.030 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Shrinkage Flow Direction 150x105x3; ISO 294-4
Shrinkage, TD 0.12 %
@Treatment Temp. 120 °C,
Time 14400 sec
150x105x3; ISO 294-4
 
Processing PropertiesOriginal ValueComments
Melt Temperature 280 °Cinjection molding
 270 - 290 °C
Mold Temperature 80.0 °Cinjection molding
 80.0 - 120 °C
Drying Temperature 80.0 °C
Dry Time 2.00 - 6.00 hour
Moisture Content 0.030 - 0.12 %Karl Fischer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Durethan® DP BKV 30 XF 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Dry
Envalior TEPEX® dynalite 102-RG600(x)/47% Roving Glass – PA 6 Consolidated Composite Laminate
Envalior Durethan® BKV 30 H2.0 000000 Nylon 6 (PA6), 30% Glass Fiber Reinforced, Dry
Envalior TEPEX® dynalite 201-C200(x)/45% Carbon – PA6.6 Consolidated Composite Laminate
Envalior TEPEX® dynalite 104-RG600(x)/47% Roving Glass – PP Consolidated Composite Laminate

PLANW9374 / 208195

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.