MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lubrizol Estane® 2102-55D Thermoplastic Polyurethane Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: Formerly Pellethane

Feature: Load-bearing capacity

Available in Americas, Europe, Middle East, Africa, India and Asia

Data provided by Lubrizol.

Lubrizol acquired the Pellethane product line from Dow in 2009.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.21 g/cc0.0437 lb/in³ASTM D792
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0060 - 0.0090 cm/cm0.0060 - 0.0090 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 5858ASTM D2240
Tensile Strength, Ultimate 49.5 MPa7180 psiASTM D412
Elongation at Break 415 %415 %ASTM D412
50% Modulus 15.3 MPa
@Strain 50 %
15.3 MPa
@Strain 50 %
ASTM D412
100% Modulus 16.2 MPa
@Strain 100 %
2350 psi
@Strain 100 %
ASTM D412
300% Modulus 35.9 MPa
@Strain 300 %
5210 psi
@Strain 300 %
ASTM D412
Flexural Modulus 0.172 GPa24.9 ksiASTM D790
Tear Strength 179 kN/m1020 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 6060H22 Wheel, 1000g; ASTM D1044
Compression Set  25 %
@Temperature 25.0 °C,
Time 79200 sec
25 %
@Temperature 77.0 °F,
Time 22.0 hour
ASTM D395, Method B
 27 %
@Temperature 70.0 °C,
Time 79200 sec
27 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395, Method B
Tensile Set 30 %30 %Elongation set after break; ASTM D412
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 135 µm/m-°C
@Temperature 20.0 °C
75.0 µin/in-°F
@Temperature 68.0 °F
ASTM D636
Vicat Softening Point 118 °C244 °F120°C/hr, 9.8N; ASTM D1525
 
Processing PropertiesMetricEnglishComments
Melt Temperature 204 - 221 °C399 - 430 °FMolding
Mold Temperature 16.0 - 60.0 °C60.8 - 140 °F
Drying Temperature 88.0 - 104 °C190 - 219 °Fair dew point <-40°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow Pellethane® 2354-55D Polyurethane Elastomer, Polyester Polycaprolactone Based
Lubrizol Estane® 2102-75A Thermoplastic Polyurethane Elastomer
Lubrizol Estane® 2102-65D Thermoplastic Polyurethane Elastomer
Lubrizol Estane® 2103-55D Thermoplastic Polyurethane Elastomer
Lubrizol Estane® 2103-65D Thermoplastic Polyurethane Elastomer

PDW256a / 138252

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.