MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow Pellethane® 2354-55D Polyurethane Elastomer, Polyester Polycaprolactone Based  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: PELLETHANE® 2354-55D is elastomer is a polyester polycaprolactone based polyurethane elastomer used in automotive applications. It allows fast molding, and once molded can be painted with polyurethane and acrylic enamels or water based elastomeric paints without a primer.

Data provided by Dow Chemical.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.21 g/cc0.0437 lb/in³
Linear Mold Shrinkage 0.010 cm/cm0.010 in/in
Melt Flow 22 g/10 min
@Load 2.16 kg,
Temperature 224 °C
22 g/10 min
@Load 4.76 lb,
Temperature 435 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 5656
Tensile Strength at Break 37.9 MPa5500 psi
Elongation at Break 460 %460 %
50% Modulus 11.0 MPa
@Strain 50 %
11.0 MPa
@Strain 50 %
100% Modulus 12.1 MPa
@Strain 100 %
1750 psi
@Strain 100 %
300% Modulus 24.8 MPa
@Strain 300 %
3600 psi
@Strain 300 %
Secant Modulus 0.138 GPa20.0 ksi2% Secant Modulus
Tear Strength 149 kN/m850 pli
Taber Abrasion, mg/1000 Cycles 4040H22 Wheel
Compression Set  30 %
@Temperature 23.0 °C
30 %
@Temperature 73.4 °F
 33 %
@Temperature 70.0 °C
33 %
@Temperature 158 °F
Tensile Set 80 %80 %Elongation set after break
 
Thermal PropertiesMetricEnglishComments
CTE, linear 135 µm/m-°C
@Temperature 20.0 °C
75.0 µin/in-°F
@Temperature 68.0 °F
Vicat Softening Point 121 °C250 °F
Clash Berg Stiffness Temperature -5.00 °C23.0 °F

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lubrizol Estane® 2102-55D Thermoplastic Polyurethane Elastomer
Lubrizol Pellethane® 2363-55DE Thermoplastic Polyurethane Elastomer
Lubrizol Pellethane® 2363-55D Thermoplastic Polyurethane Elastomer
Dow Pellethane® 2354-65D Polyurethane Elastomer, Polyester Polycaprolactone Based
Dow Pellethane® 2351-85AE Polyurethane Elastomer, Ether Based

PDW278 / 34446

Polyurethane

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.