MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow Pellethane® 2354-55D Polyurethane Elastomer, Polyester Polycaprolactone Based  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: PELLETHANE® 2354-55D is elastomer is a polyester polycaprolactone based polyurethane elastomer used in automotive applications. It allows fast molding, and once molded can be painted with polyurethane and acrylic enamels or water based elastomeric paints without a primer.

Data provided by Dow Chemical.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.21 g/cc
Linear Mold Shrinkage 0.010 cm/cm
Melt Flow 22 g/10 min
@Load 2.16 kg,
Temperature 224 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 56
Tensile Strength at Break 37.9 MPa
Elongation at Break 460 %
50% Modulus 0.0110 GPa
@Strain 50 %
100% Modulus 0.0121 GPa
@Strain 100 %
300% Modulus 0.0248 GPa
@Strain 300 %
Secant Modulus 0.138 GPa2% Secant Modulus
Tear Strength 149 kN/m
Taber Abrasion, mg/1000 Cycles 40H22 Wheel
Compression Set 30 %
@Temperature 23.0 °C
 33 %
@Temperature 70.0 °C
Tensile Set 80 %Elongation set after break
 
Thermal PropertiesOriginal ValueComments
CTE, linear 135 µm/m-°C
@Temperature 20.0 °C
Vicat Softening Point 121 °C
Clash Berg Stiffness Temperature -5.00 °C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lubrizol Estane® 2102-55D Thermoplastic Polyurethane Elastomer
Lubrizol Pellethane® 2363-55DE Thermoplastic Polyurethane Elastomer
Lubrizol Pellethane® 2363-55D Thermoplastic Polyurethane Elastomer
Dow Pellethane® 2354-65D Polyurethane Elastomer, Polyester Polycaprolactone Based
Dow Pellethane® 2351-85AE Polyurethane Elastomer, Ether Based

PDW278 / 34446

Polyurethane

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.