MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Formosa Plastics Formolene® HP4525 High Density Polyethylene
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Pipe Grade

Material Notes: Formolene® HP4525 is a high performance copolymer designed for non-pressure pipe applications. It has good long-term hoop strength performance and outstanding toughness even at low temperatures. It provides an excellent balance of stiffness, and processability in conduit pipe applications. Formolene HP4525 meets the requirements of ASTM F2160, UL651A and NEMA TC-7. DP4525A also meets a minimum ASTM D3350 Cell Classification of 335430A.

Suggested Applications: Conduit Pipe, Telecommunications Pipe, Drip Irrigation Pipe.

Information provided by Formosa Plastics.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.948 g/ccASTM D1505
ESCR 100% Igepal® >= 192 hourCondition C, F20; ASTM D1693
ESCR 10% Igepal® >= 96 hourCondition B, F10; ASTM D1693
Melt Flow 0.30 g/10 min
@Load 2.16 kg,
Temperature 190 °C
Condition E; ASTM D1238
 20 g/10 min
@Load 21.6 kg,
Temperature 190 °C
Condition E (HLMI); ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 68ASTM D2240
Tensile Strength at Break 3500 psi2 in/min, Type IV Bar; ASTM D638
Elongation at Break >= 600 %2 in/min, Type IV bar; ASTM D638
Flexural Modulus 120000 psiTangent. 16:1 span:depth, 0.5 in./min.; ASTM D790
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -175 °FASTM D746

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Formosa Plastics Formolene® HB6007F High Density Polyethylene
Formosa Plastics Formolene® HB5202B2 Sheet and Thermoforming HDPE
Formosa Plastics Formolene® E6210C High Density Polyethylene
Formosa Plastics Formolene® E6210A High Density Polyethylene
Formosa Plastics Formolene® 6575N Impact Copolymer Polypropylene

PFPCPQ9005 / 239826

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.