MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Domo TechnylStar™ SX 218 V50 PA6, 50% glass filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 50% Glass Fiber Filled

Material Notes: TECHNYLSTAR™ SX 218 V50 is based on a patented high flow polyamide 6 resin (Technylstar), heat stabilized, reinforced with 50% of glass fiber, for injection molding. This product is available in black color.

Benefits: Due to its outstanding flow characteristics, the product allows more freedom in mould and part design versus a standard polyamide solutions.

Available in: Asia Pacific, Europe and North America

Regulations compliance: Grades produced or imported in Europe comply with directive 453/2010/EC, which amends REACH directive 1907/2006/EC. This grade complies with RoHS directive 2002/95/EC. Unless specified, this grade is not suitable for food contact, medical devices or toy applications.

Applications: It is used in a wide variety of industries. The product is particularly suitable for all applications where a high rigidity is required.

Product data for dry samples.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.55 g/ccISO 1183/A
Water Absorption 0.72 %
@Temperature 23.0 °C,
Time 86400 sec
ISO 62
Viscosity 100 cP
@Shear Rate 1000 1/s,
Temperature 270 °C
 110 cP
@Shear Rate 1000 1/s,
Temperature 250 °C
 140 cP
@Shear Rate 1000 1/s,
Temperature 230 °C
 220 cP
@Shear Rate 100 1/s,
Temperature 270 °C
 300 cP
@Shear Rate 100 1/s,
Temperature 250 °C
 400 cP
@Shear Rate 100 1/s,
Temperature 230 °C
Linear Mold Shrinkage 0.0076 cm/cmIsotropy
Linear Mold Shrinkage, Flow 0.0025 cm/cm
Linear Mold Shrinkage, Transverse 0.0033 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 230 MPaISO 527 Type 1A
Tensile Stress at Strain 25.0 MPa
@Strain 0.5 %
 140 MPa
@Strain 1 %
 210 MPa
@Strain 2 %
Elongation at Break 2.5 %ASTM D638
 2.6 %ISO 527 Type 1A
Tensile Modulus 17000 MPaISO 527 Type 1A
Flexural Strength 320 MPaISO 178
Flexural Modulus 14000 MPaASTM D790
 15500 MPaISO 178
Izod Impact, Notched 180 J/mASTM D256
Izod Impact, Notched (ISO) 15.0 kJ/m²ISO 180/1eA
Izod Impact, Unnotched (ISO) 90.0 kJ/m²ISO 180/1eU
Charpy Impact Unnotched 85.0 kJ/m²ISO 179/1eU
Charpy Impact, Notched 15.0 kJ/m²ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Melting Point 222 °CISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 210 °CISO 75/Af
Flammability, UL94 HB
@Thickness 3.20 mm
1210
 
Processing PropertiesOriginal ValueComments
Feed Temperature 230 - 235 °C
Mold Temperature 80.0 - 100 °C
Drying Temperature 80.0 °C
Moisture Content <= 0.20 %
 
Descriptive Properties
Compression Zone235-240°C
Mixing Zone240-245°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Durethan® BKV 60 H2.0 EF DUS060 900116 Nylon 6 (PA6), 60% Glass Fiber Reinforced, Conditioned
Domo TechnylStar™ SX 216 V50 PA6, 50% glass filled, DRY
Domo TechnylStar™ SX 218 V50 BK 38N-K PA6, 50% glass filled, DRY
Domo TechnylStar™ SX 218 L2 V60 Black JA6A PA6, 60% glass filled, DRY
Domo TechnylStar™ AFX 218 V50 PA6, 50% glass filled

PRHOD847 / 138078

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.