MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Elix Polymers ELIX ABS P3H-AT Acrylonitrile Butadiene Styrene (ABS)
Categories: Polymer; Thermoplastic; ABS Polymer

Material Notes: Improved chemical and dynamic resistance, high gloss, contains antistatic additive

ISO Shortname: ISO 2580-1 -ABS 0, MGZ, 095-08-16-25

Information provided by Elix Polymers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm60x60x2; ISO 294-4
Linear Mold Shrinkage, Flow 0.0040 - 0.0070 cm/cm60x60x2; ISO 294-4
Melt Flow 12 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 105 MPaISO 2039-1
Tensile Strength, Yield 48.0 MPa50 mm/min; ISO 527-1,-2
Elongation at Break >= 15 %50 mm/min; ISO 527-1,-2
Elongation at Yield 2.4 %50 mm/min; ISO 527-1, -2
Tensile Modulus 2500 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 71.0 MPa2 mm/min; ISO 178
Flexural Modulus 2400 MPa2 mm/min; ISO 178
Izod Impact, Notched (ISO) 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180-1A
 18.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
Charpy Impact Unnotched 90.0 kJ/m²
@Temperature -30.0 °C
ISO 179-1eU
 180 kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
Charpy Impact, Notched 11.0 kJ/m²
@Temperature -30.0 °C
ISO 179-1eA
 20.0 kJ/m²
@Temperature 23.0 °C
ISO 179-1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+15 ohmIEC 60093
Dielectric Constant 2.9
@Frequency 1e+6 Hz
IEC 60250
 3.1
@Frequency 100 Hz
IEC 60250
Dielectric Strength 33.0 kV/mm
@Thickness 1.00 mm
IEC 60243-1
Dissipation Factor 0.060
@Frequency 100 Hz
IEC 60250
 0.080
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 90.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Deflection Temperature at 0.46 MPa (66 psi) 96.0 °CISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 92.0 °CISO 75-1,-2
Vicat Softening Point 96.0 °C
@Load 5.10 kg
50°C/h; ISO 306
Flammability, UL94 HB
@Thickness 1.60 mm
Glow Wire Flammability Index 650 °C
@Thickness 2.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 240 °CInjection molding; ISO 294
Mold Temperature 70.0 °CInjection molding; ISO 294
Injection Velocity 240 mm/secInjection molding; ISO 294
 
Descriptive Properties
Burning rate50 mm/minUS-FMVSS, ISO 3795, 2 mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Elix Polymers Elix™ 114 H ABS Polymer Modifier
Elix Polymers ELIX PC/ABS 5130 Polycarbonate/ABS Alloy
Elix Polymers ELIX ABS H701 Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, High Impact
Elix Polymers Cadon CG 28 ABS Copolymer
Celanese Zytel® 70G30L NC010 PA66-GF30

PELIX003 / 183318

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.