MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LyondellBasell Ultrathene® UE637000 Ethylene Vinyl Acetate Copolymer, Film Extrusion Grade
Categories: Polymer; Film; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Film Grade

Material Notes: ULTRATHENE UE637000 is an EVA copolymer with good toughness, flexibility and clarity. Applications include laminating and heavy duty films as well as injection and blow molding. UE637000 contains no additives.

Regulatory Status: The basic copolymer UE637000 meets the requirements of the Food and Drug Administration regulations 21 CFR 177.1350 and 21 CFR 175.105. These regulations (respectively) allow for the use of this material as articles or components of articles which are "...intended for use in producing, manufacturing, packing, processing, preparing, treating, packaging, transporting or holding food..." and as an adhesive which "...may be safely used as components of articles intended for use in packaging, transporting or holding food." Specific limitations or conditions of use may apply..

Processing Techniques: The maximum recommended melt temperature for UE637000 is 430°F (221°C).

This product is from the former Equistar product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Vinyl Acetate Content 9.0 %
Thickness 2.00 mil
Melt Flow 3.2 g/10 minASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 94ASTM D2240
Film Tensile Strength at Yield, MD 904 psiASTM D882
Film Tensile Strength at Yield, TD 843 psiASTM D882
Film Elongation at Break, MD 350 %ASTM D882
Film Elongation at Break, TD 500 %ASTM D882
Film Elongation at Yield, MD 9.0 %ASTM D882
Film Elongation at Yield, TD 11 %ASTM D882
Dart Drop 202 g/milF50; ASTM D4272
Film Tensile Strength at Break, MD 3750 psiASTM D882
Film Tensile Strength at Break, TD 2740 psiASTM D882
1% Secant Modulus, MD 12300 psiASTM D882
1% Secant Modulus, TD 13200 psiASTM D882
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 80.0 °CASTM D1525
Brittleness Temperature <= -76.0 °CASTM D746
 
Processing PropertiesOriginal ValueComments
Melt Temperature <= 430 °F
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LyondellBasell Petrothene® NA247000 Low Density Polyethylene, Injection Molding Grade
LyondellBasell Ultrathene® UE624000 Ethyl Vinyl Acetate Copolymer
Eurofoam Evacell EVA 30 EVA + PE Foam
Versalis Greenflex® FD 53 Ethylene Vinyl Acetate Copolymer - Blown Film Extrusion
Eurofoam Evacell EVA 100 EVA + PE Foam

PEQU0811 / 104167

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.