MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese FORTRON 320 PPS, Unfilled
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS)

Material Notes: 0320 exhibits a high melt strength for extrusion processes. The material demonstrates excellent heat and chemical resistance. The intended use of this product is for extruding monofilament/fibers, rod and slab. Available standard in powder (0320B0), pellet (0320P0) and crystallized pellet (0320C0) form.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.40 g/cc1.40 g/ccASTM D792
Density 1.35 g/cc0.0488 lb/in³ISO 1183
Water Absorption at Saturation 0.020 %0.020 %ISO 62
Linear Mold Shrinkage, Flow 0.010 - 0.012 cm/cm0.010 - 0.012 in/inASTM D955
 0.012 - 0.015 cm/cm0.012 - 0.015 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0080 - 0.010 cm/cm0.0080 - 0.010 in/inASTM D955
 0.015 - 0.018 cm/cm0.015 - 0.018 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 9090ISO 2039-2
 9393ASTM D785
Tensile Strength at Break 90.0 MPa13100 psi5mm/min; ISO 527-2/1A
Elongation at Break 8.0 %8.0 %5mm/min; ISO 527-2/1A
Tensile Modulus 3.50 GPa508 ksi50mm/min; ISO 527-2/1A
Flexural Strength 145 MPa21000 psiISO 178
Flexural Modulus 4.20 GPa609 ksiISO 178
Izod Impact, Notched (ISO)  2.50 kJ/m²
@Temperature -30.0 °C
1.19 ft-lb/in²
@Temperature -22.0 °F
ISO 180/1A
 82.0 kJ/m²
@Temperature 23.0 °C
39.0 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1U
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+7 ohm-cm1.00e+7 ohm-cmASTM D257
 1.00e+11 ohm-cm1.00e+11 ohm-cmIEC 60093
Dielectric Constant  3.0
@Frequency 1000 Hz
3.0
@Frequency 1000 Hz
ASTM D150
 3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
ASTM D150
 4.6
@Frequency 1e+6 Hz
4.6
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 17.7 kV/mm450 kV/inshort term; ASTM D149
 18.0 kV/mm457 kV/inIEC 60243-1
Dissipation Factor  0.00090
@Frequency 1e+6 Hz
0.00090
@Frequency 1e+6 Hz
ASTM D150
 0.0010
@Frequency 1000 Hz
0.0010
@Frequency 1000 Hz
ASTM D150
 0.0011
@Frequency 1e+6 Hz
0.0011
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 124 sec124 secASTM D495
Comparative Tracking Index 125 V125 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 52.0 µm/m-°C28.9 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 53.0 µm/m-°C29.4 µin/in-°FISO 11359-2
Specific Heat Capacity 1.83 J/g-°C0.437 BTU/lb-°F
Melting Point 280 °C536 °F10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 204 °C400 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 104 °C220 °FASTM D648
 115 °C239 °FISO 75-1, -2
Deflection Temperature at 8.0 MPa 95.0 °C203 °FISO 75-1, -2
Glass Transition Temp, Tg 90.0 °C194 °FISO 11357-1,-2,-3
Flammability, UL94 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 140 - 160 °C284 - 320 °Fcavity
 310 - 320 °C590 - 608 °Fhot runner
Feed Temperature 60.0 - 80.0 °C140 - 176 °F
Zone 1 290 - 300 °C554 - 572 °F
Zone 2 300 - 310 °C572 - 590 °F
Zone 3 310 - 320 °C590 - 608 °F
Zone 4 310 - 320 °C590 - 608 °F
Die Temperature 300 - 310 °C572 - 590 °F
Melt Temperature 310 - 320 °C590 - 608 °F
Drying Temperature 110 - 120 °C230 - 248 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour
Moisture Content <= 0.020 %<= 0.020 %
Injection Pressure 40.0 - 80.0 MPa5800 - 11600 psi
Hold Pressure 30.0 - 60.0 MPa4350 - 8700 psi
Back Pressure <= 3.00 MPa<= 435 psi
Screw Speed  50 rpm
@Diameter 55.0 mm
50 rpm
@Diameter 2.17 in
 75 rpm
@Diameter 40.0 mm
75 rpm
@Diameter 1.57 in
 120 rpm
@Diameter 25.0 mm
120 rpm
@Diameter 0.984 in
 
Descriptive Properties
Injection moldingYes
Injection speedfast
Sheet extrusionYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese FORTRON 203 PPS, Unfilled
Celanese FORTRON 214 PPS, Unfilled
Celanese FORTRON 205 PPS, Unfilled
Celanese FORTRON 309 PPS, Unfilled
Celanese FORTRON 0205B4/20µm PPS, Specialty

PHCQ263 / 178718

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.