MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Flame Retardant adhesives

(Viewing data as-entered. Click here to return)
Sumitomo Bakelite North America RX® 640 Fiberglass Reinforced Phenolic Resole
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Phenolic; Phenolic, Resole, Glass Fiber Filled

Material Notes: RX® 640 is a fiberglass reinforced, ammonia-free, phenolic resole compound, with good dimensional stability and good strength at elevated temperatures. Meets ASTM D-5948 Type GPI-5.

Information supplied by Sumitomo Bakelite North America.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.80 g/ccPowder; ASTM D1895
Density 1.76 g/ccASTM D792
Water Absorption 0.06 %
@Time 86000 sec
ASTM D570
 0.22 %
@Time 170000 sec
ASTM D570
Linear Mold Shrinkage 0.002 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell E 90ASTM D785
Tensile Strength, Ultimate 86 MPaISO 527
Flexural Strength 186 MPaISO 178
Flexural Modulus 14.5 GPaISO 178
Compressive Strength 248 MPaISO 604
Charpy Impact, Notched 0.40 J/cm²ISO 179
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 11.8 kV/mm
@Frequency 60 Hz
Wet, step-by-step; ASTM D149
 14.0 kV/mm
@Frequency 60 Hz
Wet, short time; ASTM D149
Arc Resistance 160 secASTM D495
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 14.0 µm/m-°C
@Temperature 23.0 °C
TMA; ASTM E381
Thermal Conductivity 0.550 W/m-KASTM F433
Maximum Service Temperature, Air 150 °CUL Temperature Index; UL 746B
Deflection Temperature at 1.8 MPa (264 psi) 280 °CAs Molded; ASTM D648A
 >= 282 °CPost Baked; ISO 75 A
Flammability, UL94 V-0
@Thickness 1.60 mm
 V-0
@Thickness 3.20 mm
 
Descriptive Properties
Available Molding GradesCompression, Transfer, Injection
ColorBlack
FormGranular

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sumitomo Bakelite RX® 643 Phenolic Resole Compound
Sumitomo Bakelite RX® 647 Phenolic Resole Compound
Sumitomo Bakelite Durez® 118 Phenolic, Compression Grade
Sumitomo Bakelite Durez® 32962 Phenolic Molding Compound, Compression Grade
Sumitomo Bakelite North America RX® 853G Fiberglass Reinforced Phenolic Novolac

P90XR03 / 21217

Flame Retardant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.