MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Selenium, Se
Categories: Metal; Nonferrous Metal; Other Engineering Material; Semiconductor; Pure Element

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 3.91 g/cc
@Temperature 406 °C
Liquid
 3.975 g/cc
@Temperature 217 °C
Liquid
 4.02 g/cc
@Temperature 305 °C
Liquid
 4.06 g/cc
@Temperature 267 °C
Liquid
 4.28 g/cc
@Temperature 20.0 °C
Vitreous
 4.389 g/cc
@Temperature 25.0 °C
alpha phase
 4.47 g/cc
@Temperature 25.0 °C
beta phase
 4.809 g/cc
@Temperature 25.0 °C
gamma phase
a Lattice Constant 4.36 ÅGray Selenium
c Lattice Constant 4.95 ÅGray Selenium
Vapor Pressure 0.001013 bar
@Temperature 344 °C
 0.01013 bar
@Temperature 431 °C
 0.1013 bar
@Temperature 540 °C
 1.013 bar
@Temperature 684.9 °C
Surface Tension 98 dynes/cm
@Temperature 280 °C
 98.2 dynes/cm
@Temperature 310 °C
 100.5 dynes/cm
@Temperature 250 °C
 105.5 dynes/cm
@Temperature 220 °C
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 78.961995
Atomic Number 34
Thermal Neutron Cross Section 11.8 barns/atom
X-ray Absorption Edge 0.979 ÅK
 7.467 ÅLI
 8.4212 ÅLII
 8.6624 ÅLIII
Critical Temperature 1493 °CGray Se
Electronegativity 2.55Pauling
Ionic Radius 0.420 ÅCrystal Ionic Radius for Valence +6
 0.500 ÅCrystal Ionic Radius for Valence +4
 0.660 ÅCrystal Ionic Radius for Valence +1
 1.91 ÅCrystal Ionic Radius for Valence -2
 2.32 ÅCrystal Ionic Radius for Valence -1
Electrochemical Equivalent 0.50 g/A/h
 
Mechanical PropertiesOriginal ValueComments
Knoop Microhardness 350N/mm² Microhardness Gray Selenium
Modulus of Elasticity 57.9 GPa
Shear Modulus 6.46 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000120 ohm-cm
Magnetic Susceptibility -0.0000221Gray Selenium; Atomic (cgs)
 -3.20e-7cgs/g
Critical Superconducting Temperature 6.75 - 6.95 K6.75, 6.95 at ~13.0 GPa pressure for Se II
Dielectric Constant 6.6
@Frequency 1e+8 Hz
Gray Selenium
Band Gap 1.5 eVGray Selenium
Hole Mobility, cm²/V-s 5.0Gray Selenium
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 84.0 J/g
Heat of Vaporization 3140 J/g
CTE, linear 17.89 µm/m-°C
@Temperature 20.0 °C
Gray Selenium, Perpendicular to c-axis
 37.0 µm/m-°C
@Temperature 20.0 - 100 °C
vitreous Se
 49.0 µm/m-°C
@Temperature 20.0 - 100 °C
for gamma Se
 74.1 µm/m-°C
@Temperature 20.0 °C
Gray Selenium; Parallel to c-axis
Specific Heat Capacity 0.2926 J/g-°CGray Selenium
 0.352 J/g-°C
Thermal Conductivity 1.31 W/m-KGray Selenium; Parallel to c-axis
 2.90 W/m-K
 4.52 W/m-KGray Selenium; Perpendicular to c-axis
Melting Point 220 °C
Boiling Point 685 °C
 
Optical PropertiesOriginal ValueComments
Refractive Index 2.50Gray Selenium
 
Component Elements PropertiesOriginal ValueComments
Selenium, Se 100 %
 
Descriptive Properties
CAS Number7782-49-2

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Germanium, Ge
Silicon, Si
Tellurium, Te
Silver, Ag
Aluminum, Al

AMESe00 / 101

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.