MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
GEHR Plastics PVDF Polyvinylidene Fluoride
Categories: Polymer; Thermoplastic; Fluoropolymer; Polyvinylidene Fluoride (PVDF)

Material Notes: Polyvinylidene fluoride shows a higher tensile strength, pressure resistance and dimensional stability than the related PTFE, but friction and insulation properties are lower. PVDF has a high mechanical strength and toughness at lower temperature and it's self-extinguishing. The temperature ranges from -30°C to 150°C.

Properties

  • high tensile strength
  • high mechanical strength
  • high rigidity
  • high chemical resistance
  • very low water absorption
  • good friction and wear and tear values
  • self-extinguishing
  • high UV-resistance
  • toxic fumes when burned
  • can not be solvent cemented
  • relatively high coefficient of thermal expansion
Applications include gaskets, pumps, rotation disks, valves, flap traps, centrifugals of extraction, fittings, glide tracks, and cogwheels.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.78 g/ccISO 1183
Moisture Absorption at Equilibrium 0.010 %ISO 62
Water Absorption at Saturation 0.040 %ISO 62
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 80ISO 868
Ball Indentation Hardness 120 MPaISO 2039
Tensile Strength at Break 46.0 MPaISO 527
Tensile Strength, Yield 58.0 MPaISO 527
Elongation at Break 29 %ISO 527
Elongation at Yield 17 %ISO 527
Modulus of Elasticity 2.125 GPaISO 527
Flexural Strength 80.0 MPaISO 178
Charpy Impact Unnotched NBISO 179
Charpy Impact, Notched 12.0 kJ/m²ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 3.00e+10 ohm-cmIEC 60093
Surface Resistance >= 1.00e+13 ohmIEC 60093
Dielectric Constant 7.0
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 27.0 kV/mmIEC 60243-1
Dielectric Loss Index 0.24
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 130 µm/m-°CISO 11359
Thermal Conductivity 0.130 W/m-K
@Temperature 20.0 °C
ISO 22007-4
Melting Point 171 °CDIN EN ISO 3146
Maximum Service Temperature, Air 150 °CUL 746B
Deflection Temperature at 0.46 MPa (66 psi) 145 °CISO 75
Deflection Temperature at 1.8 MPa (264 psi) 104 °CISO 75
Vicat Softening Point 138 °CVST/B/50; ISO 306
 160 °CVST/A/50; ISO 306
Minimum Service Temperature, Air -30.0 °CUL 746B
Glass Transition Temp, Tg -40.0 °CDIN EN ISO 3146
Flammability, UL94 V-0UL 94
Oxygen Index 44 %ASTM D2863
 
Compliance PropertiesOriginal ValueComments
FDA YesPhysiological indifference
 
Descriptive Properties
Acid Resistancelimited
Aromatic Resistanceyes
Bondabilitylimited, pretreatment necessary
CKW Resistanceyes
Colornatural
Hydrocarbonate Resistanceyes
Hydroxide Resistanceyes
Ketone Resistanceyes
Physiological indifferenceno, EEC
Resistance Against Hot Wateryes
UV Stabilizationyes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
CENTROPLAST CENTROFLON Polyvinylidene fluoride
Hippe PVDF
Adamas Lakinor® U PVDF
Delrin Delrin® 100 BK602 POM
Ensinger TECAFLON™ PVDF Polyvinylidene Fluoride - extruded products

PGEHR029 / 79866

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.