MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Titanium Ti-3Al-2.5V (Grade 9), alpha annealed
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Near Alpha Titanium Alloy

Material Notes: Information provided by Allvac and the references. Alpha annealed. High strength-to-weight ratio, lighter than stainless steel. Good corrosion resistance in mildly reducing to highly oxidizing media

Applications: Excellent cold formability, 20-50% higher tensile properties than CP titanium grades. Primarily used in aircraft hydraulic systems.

Forms typically available: Sheet, strip, foil and tubing.

3 other heat treatments of this alloy are in MatWeb.

Key Words: Ti3Al2.5V, UNS R56320; ASTM Grade 9; Half 6-4; Tubing Alloy
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 4.48 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 256Estimated from Rockwell C.
Hardness, Knoop 278Estimated from Rockwell C.
Hardness, Rockwell C 24
Hardness, Vickers 280
Tensile Strength, Ultimate 620 MPa
Tensile Strength, Yield 500 MPa
Elongation at Break 15 %
Tensile Modulus 100 GPa
 80.0 GPa
@Temperature 230 °C
Compressive Yield Strength 690 MPa
Notched Tensile Strength 790 MPaKt (stress concentration factor) = 6.3
Poissons Ratio 0.30
Fatigue Strength 170 MPa
@# of Cycles 1.00e+7
Kt (stress concentration factor) = 1.8
 280 MPa
@# of Cycles 50000
Kt (stress concentration factor) = 1.8
 280 MPa
@# of Cycles 1.00e+7
unnotched
 380 MPa
@# of Cycles 40000
unnotched
Fracture Toughness 100 MPa-m½kJ/m² for J(IC)
Shear Modulus 44.0 GPa
Charpy Impact 86.0 JV-notch
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000127 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.61 µm/m-°C
@Temperature 20.0 - 95.0 °C
 9.67 µm/m-°C
@Temperature 20.0 - 205 °C
 9.86 µm/m-°C
@Temperature 20.0 - 315 °C
 9.97 µm/m-°C
@Temperature 20.0 - 540 °C
average
Specific Heat Capacity 0.525 J/g-°CTypical value for titanium alloys.
Thermal Conductivity 8.30 W/m-K
@Temperature 23.0 °C
 11.8 W/m-K
@Temperature 315 °C
Melting Point <= 1700 °C
Solidus 1704 °C
Liquidus 1700 °C
Beta Transus 935 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 2.5 - 3.5 %
Carbon, C <= 0.050 %
Hydrogen, H <= 0.015 %
Iron, Fe <= 0.20 %
Nitrogen, N <= 0.030 %
Other, each <= 0.050 %
Other, total <= 0.30 %
Oxygen, O <= 0.15 %
Titanium, Ti 92.755 - 95.5 %As Balance; Elemental Composition per ASTM B265
Vanadium, V 2.0 - 3.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Titanium Ti-3Al-2.5V (Grade 9), Alpha-Beta Anneal, Quenched
Titanium Ti-3Al-2.5V (Grade 9), ST 925°C, Aged 480°C (900°F)
Titanium Ti-3Al-2.5V (Grade 9), Beta-Anneal 950°C
Titanium Ti-6Al-4V (Grade 5), Annealed
Aluminum 6061-T6; 6061-T651

MTA321 / 14123

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.