MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI 1118 Steel, cold drawn, low temperature, stress relieved, round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Low Carbon Steel

Material Notes: Applications include medium duty shafts, studs, pins, distributor cams, cam shafts, and universal joints.

Key Words: NS G11180, ASTM A29, ASTM A107, ASTM A108, FED QQ-S-637 (C1118), SAE J403, SAE J412, SAE J414
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.87 g/ccTypical for steel.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 131
@Diameter 50.8 - 76.2 mm
 143
@Diameter 31.8 - 50.8 mm
 149
@Diameter 22.2 - 31.8 mm
 163
@Diameter 15.9 - 22.2 mm
Hardness, Knoop 150
@Diameter 50.8 - 76.2 mm
Converted from Brinell
 163
@Diameter 31.8 - 50.8 mm
Converted from Brinell
 169
@Diameter 22.2 - 31.8 mm
Converted from Brinell
 184
@Diameter 15.9 - 22.2 mm
Converted from Brinell
Hardness, Rockwell B 73
@Diameter 50.8 - 76.2 mm
Converted from Brinell
 78
@Diameter 31.8 - 50.8 mm
Converted from Brinell
 80
@Diameter 22.2 - 31.8 mm
Converted from Brinell
 84
@Diameter 15.9 - 22.2 mm
Converted from Brinell
Hardness, Vickers 136
@Diameter 50.8 - 76.2 mm
Converted from Brinell
 149
@Diameter 31.8 - 50.8 mm
Converted from Brinell
 155
@Diameter 22.2 - 31.8 mm
Converted from Brinell
 170
@Diameter 15.9 - 22.2 mm
Converted from Brinell
Tensile Strength, Ultimate 450 MPa
@Diameter 50.8 - 76.2 mm
 485 MPa
@Diameter 31.8 - 50.8 mm
 515 MPa
@Diameter 22.2 - 31.8 mm
 550 MPa
@Diameter 15.9 - 22.2 mm
Tensile Strength, Yield 380 MPa
@Diameter 50.8 - 76.2 mm
 415 MPa
@Diameter 31.8 - 50.8 mm
 450 MPa
@Diameter 22.2 - 31.8 mm
 485 MPa
@Diameter 15.9 - 22.2 mm
Elongation at Break 12 %
@Diameter 50.8 - 76.2 mm
in 50 mm
 13 %
@Diameter 31.8 - 50.8 mm
in 50 mm
 15 %
@Diameter 15.9 - 22.2 mm
in 50 mm
 15 %
@Diameter 22.2 - 31.8 mm
in 50 mm
Reduction of Area 35 %
@Diameter 31.8 - 50.8 mm
 35 %
@Diameter 50.8 - 76.2 mm
 40 %
@Diameter 15.9 - 22.2 mm
 40 %
@Diameter 22.2 - 31.8 mm
Modulus of Elasticity 200 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steel.
Poissons Ratio 0.29Typical For Steel
Shear Modulus 80.0 GPaTypical for steel.
Izod Impact 103 Jnormalized at 925°C (1700°F)
 107 Jannealed at 790°C (1450°F)
 108 Jas rolled
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000174 ohm-cmTypical steel
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.5 µm/m-°C
@Temperature 20.0 °C
Typical steel
 12.2 µm/m-°C
@Temperature 0.000 - 300 °C
Typical for steel
 13.9 µm/m-°C
@Temperature 0.000 - 500 °C
Typical for steel
Specific Heat Capacity 0.472 J/g-°CTypical steel
Thermal Conductivity 51.9 W/m-KTypical steel
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.14 - 0.20 %
Iron, Fe 98.03 - 98.48 %As remainder
Manganese, Mn 1.3 - 1.6 %
Phosphorus, P <= 0.040 %
Sulfur, S 0.080 - 0.13 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1117 Steel, cold drawn, low temperature, stress relieved, round
AISI 1118 Steel, cold drawn, high temperature, stress relieved, round
AISI 1117 Steel, as cold drawn, 22-32 mm (0.875-1.25 in) round
AISI 1118 Steel, as cold drawn, round
AISI 1117 Steel, cold drawn, high temperature, stress relieved, round

M1118H / 7161

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.