MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LATI Larpeek 10 GCE/600 PEEK, Glass/Mineral Reinforced
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Glass Fiber Filled

Material Notes: Polyetheretherketone (PEEK) based compound. Glass fibers / Mineral filler. Very good chemical resistance. Very good thermal properties. Low smoke density and low toxicity index.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Information provided by Lati Industria Termoplastici S.p.A.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.93 g/cc0.0697 lb/in³
Linear Mold Shrinkage, Flow 0.0020 - 0.0045 cm/cm0.0020 - 0.0045 in/in
Linear Mold Shrinkage, Transverse 0.0030 - 0.0050 cm/cm0.0030 - 0.0050 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break  100 MPa
@Temperature 150 °C
14500 psi
@Temperature 302 °F
 115 MPa
@Temperature 120 °C
16700 psi
@Temperature 248 °F
 135 MPa
@Temperature 90.0 °C
19600 psi
@Temperature 194 °F
 145 MPa
@Temperature 60.0 °C
21000 psi
@Temperature 140 °F
 160 MPa
@Temperature 23.0 °C
23200 psi
@Temperature 73.4 °F
Elongation at Break  1.3 %
@Temperature 23.0 °C
1.3 %
@Temperature 73.4 °F
 1.3 %
@Temperature 60.0 °C
1.3 %
@Temperature 140 °F
 1.4 %
@Temperature 90.0 °C
1.4 %
@Temperature 194 °F
 1.4 %
@Temperature 120 °C
1.4 %
@Temperature 248 °F
 1.5 %
@Temperature 150 °C
1.5 %
@Temperature 302 °F
Tensile Modulus  15.6 GPa
@Temperature 150 °C
2260 ksi
@Temperature 302 °F
 16.0 GPa
@Temperature 120 °C
2320 ksi
@Temperature 248 °F
 16.9 GPa
@Temperature 90.0 °C
2450 ksi
@Temperature 194 °F
 17.2 GPa
@Temperature 60.0 °C
2490 ksi
@Temperature 140 °F
 17.6 GPa
@Temperature 23.0 °C
2550 ksi
@Temperature 73.4 °F
Charpy Impact Unnotched 4.00 J/cm²19.0 ft-lb/in²
Charpy Impact, Notched 0.600 J/cm²2.86 ft-lb/in²
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 200 V200 VA solution
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 250 °C482 °F
Deflection Temperature at 0.46 MPa (66 psi) >= 300 °C>= 572 °F
Deflection Temperature at 1.8 MPa (264 psi) >= 300 °C>= 572 °F
Vicat Softening Point >= 300 °C
@Load 5.00 kg
>= 572 °F
@Load 11.0 lb
Flammability, UL94  V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
 V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 390 - 400 °C734 - 752 °F
Mold Temperature 170 - 200 °C338 - 392 °F
Drying Temperature 120 - 150 °C
@Time 10800 sec
248 - 302 °F
@Time 3.00 hour
 
Descriptive Properties
ISO Shrinkage - Pressure60 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Celstran® PP-GF60-25 AD3002 Black PP, 60% Glass Reinforced
Plenco 1510 Polyester, Pellet, Injection Molded
Avient OnForce™ LFT SF-40LCF/000 Black Polyphenylene Sulfide (PPS)
Polynt 30 CF60- 6mm Carbon Fiber VE BMC
Mitsubishi Iupital® FC2020D Copolymer Acetal

PLATH9640 / 177336

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.